Aluminum scandium nitride film and ferroelectric assembly

By partially replacing aluminum with gallium in an aluminum scandium nitride film, a gallium scandium nitride film with a hexagonal wurtzite structure is formed, which solves the problems of high coercivity and low remanent polarization of aluminum scandium nitride films, and realizes a small ferroelectric component driven by low power consumption.

CN118974306APending Publication Date: 2024-11-15TOSOH CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030653.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-25
Filing Date
2023-03-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

There is still room for improvement in the reduction of coercive electric field and the increase of residual polarization in existing aluminum nitride scandium films.

Method used

By partially replacing aluminum with gallium in an aluminum scandium nitride film, a gallium scandium nitride film containing aluminum, scandium, and nitrogen is formed. Its crystal phase is controlled to be hexagonal, wurtzite-type structure, with internal parameter u less than 1.0, x greater than 0.4 and less than 0.6, y greater than 0.1 and less than 0.5, z greater than 0.1 and less than 0.3, and thickness less than 2000 nm.

Benefits of technology

It achieves the increase of residual polarization while reducing the coercive electric field, making it suitable for small ferroelectric components driven by low power consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974306A_ABST
    Figure CN118974306A_ABST
Patent Text Reader

Abstract

The aluminum-scandium nitride film according to the present invention contains aluminum, scandium, and nitrogen, and also contains gallium. The crystalline phase of the aluminum scandium nitride film may include hexagonal crystals. The crystalline phase of the aluminum nitride scandium film can be of a wurtzite type structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum scandium nitride film and a ferroelectric component. Background Art

[0002] It is well known that scandium aluminum nitride films show the highest ferroelectricity among ferroelectrics and are expected to be used in storage elements such as ferroelectric memories, or piezoelectric components such as pressure sensors and vibration sensors.

[0003] As such an aluminum scandium nitride film, for example, one described in the following Patent Document 1 is known. The following Patent Document 1 proposes to improve the ferroelectricity of the aluminum scandium nitride film by reducing the scandium concentration.

[0004] Prior art literature

[0005] Non-patent literature

[0006] Non-patent document 1: Yasuoka et al., Effect of deposition conditions on (Al 1-x Sc x Yasuoka et al., “Effects of deposition conditions on the ferroelectric properties of (Al 1-x Sc x )N thin films", j.Appl.Phys.,128,114103,2020) Summary of the invention

[0007] Problem that the invention aims to solve

[0008] However, the aluminum scandium nitride film described in Non-Patent Document 1 still has room for improvement in terms of reduction of coercive electric field and increase of remanent polarization.

[0009] An object of the present invention is to provide at least one of an aluminum scandium nitride film and a ferroelectric component having the same that can reduce a coercive electric field and increase a residual polarization.

[0010] Solutions for solving problems

[0011] The inventors of the present invention have focused on replacing part of the aluminum in an aluminum-scandium nitride film with gallium, which is in the same group as aluminum. However, they have found that a gallium-scandium nitride film in which all the aluminum is replaced with gallium has a lower remanent polarization than an aluminum-scandium nitride film. In contrast, they unexpectedly found that by replacing part of the aluminum in the aluminum-scandium nitride film with gallium, but not all of it, the remanent polarization becomes larger and the coercive field is reduced.

[0012] The present invention has been accomplished based on such findings, and the contents of the present invention are as described in the claims. In addition, the gist of the present invention is as follows.

[0013] (1) An aluminum scandium nitride film comprising aluminum, scandium, and nitrogen, and further comprising gallium.

[0014] (2) The aluminum scandium nitride film according to (1), wherein a crystal phase of the aluminum scandium nitride film includes hexagonal crystals.

[0015] (3) The aluminum scandium nitride film according to (2), wherein a crystal phase of the aluminum scandium nitride film is a wurtzite structure.

[0016] (4) The aluminum scandium nitride film according to (3), wherein an internal parameter u defined by the following formula (A) is less than 1.0.

[0017] uparameter=(a 2 / 3c 2 )+0.25(A)

[0018] (In the above formula (A), a represents the lattice constant of the a-axis c represents the lattice constant of the c-axis )

[0019] (5) The aluminum scandium nitride film according to (4), wherein the internal parameter u is greater than or equal to 0.30 and less than or equal to 0.50.

[0020] (6) The aluminum scandium nitride film according to any one of (1) to (5), wherein the aluminum scandium nitride film is represented by the following composition formula (B).

[0021] (Al x Sc y Ga z )N(B)

[0022] (In the above formula (B), x is 0.4 to 0.6, y is 0.1 to 0.5, z is 0.1 to 0.3, and x+y+z is 1.)

[0023] (7) The aluminum scandium nitride film according to any one of (1) to (6), wherein the thickness is 2000 nm or less.

[0024] (8) The aluminum scandium nitride film according to any one of (1) to (7), wherein the thickness is 250 nm or less.

[0025] (9) The aluminum scandium nitride film according to any one of (1) to (7), wherein the thickness is greater than 250 nm.

[0026] (10) A ferroelectric device comprising the aluminum scandium nitride film according to any one of (1) to (9).

[0027] Effects of the Invention

[0028] The present invention provides at least one of an aluminum scandium nitride film and a ferroelectric component that can reduce the coercive electric field and increase the residual polarization. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a cross-sectional view showing one embodiment of the ferroelectric device of the present invention.

[0030] Figure 2 This is a graph showing an X-ray diffraction profile of the scandium aluminum nitride film of Example 1 obtained by an out-of-plane method.

[0031] Figure 3 This is a graph showing an X-ray diffraction profile of the scandium aluminum nitride film of Example 1 obtained by an in-plane method. DETAILED DESCRIPTION

[0032] An embodiment of the present invention will be described in detail by giving an example. However, the present invention is not limited to the following embodiment.

[0033] <Aluminum Scandium Nitride Film>

[0034] First, an embodiment of the aluminum scandium nitride film of the present invention will be described.

[0035] The aluminum scandium nitride film contains aluminum, scandium, and nitrogen, and also contains gallium.

[0036] The aluminum scandium nitride film can reduce the coercive field and increase the residual polarization, so it can be driven with low power consumption, and it is expected to realize a small ferroelectric device.

[0037] As one of the reasons for the above effect, it can be considered that since the atomic radius of gallium is close to that of aluminum, etc., by replacing part of the aluminum or scandium of aluminum scandium nitride (AlScN) with gallium, the AlScN crystal is easily strained, the polarization is easily reversed, and as a result, the coercive electric field is reduced. In addition, as a reason for the increase in residual polarization, it can be considered that the polarization is easy to change near the coercive electric field, and the shape of the hysteresis curve is close to an ideal quadrilateral shape.

[0038] The crystalline phase of the aluminum scandium nitride film includes hexagonal crystals, preferably consists of hexagonal crystals, and more preferably has a wurtzite structure.

[0039] The aluminum scandium nitride film preferably has strain in the crystal, and the internal parameter u defined by the following formula (A) is preferably less than 1.0.

[0040] Internal parameter u=(a 2 / 3c2 )+0.25(A)

[0041] (In the above formula (A), a represents the lattice constant of the a-axis c represents the lattice constant of the c-axis )

[0042] The internal parameter u is one of the indicators of the strain of the crystal, and the smaller its value means the greater the strain. By reducing the internal parameter, the residual polarization can be further increased. The internal parameter u is preferably greater than 0.30 and less than 0.50, and more preferably greater than 0.35 and less than 0.40.

[0043] The aluminum scandium nitride film is represented by, for example, the following composition formula (B).

[0044] (Al x Sc y Ga z )N(B)

[0045] In the above formula (B), x only needs to be greater than 0 and less than 1, and is preferably greater than 0.1, greater than 0.2, greater than 0.3, or greater than 0.4. In this case, the remanent polarization (Pr) tends to be large.

[0046] Here, x is preferably 0.99 or less, and may be 0.95 or less, 0.7 or less, or 0.5 or less. In this case, the residual polarization increases, and the difference between the coercive field and the dielectric breakdown field increases.

[0047] In the above formula (B), y may be greater than 0 and less than 1, and may be 0.1 or more, 0.15 or more, 0.3 or more, or 0.4 or more.

[0048] Among them, y is preferably 0.95 or less, and may be 0.6 or less, 0.5 or less, 0.4 or less, or 0.3 or less. In this case, the coercive electric field (Ec) can be more easily reduced.

[0049] In the above formula (B), z is represented by 1-xy and may be greater than 0 and less than 1, and is more preferably greater than 0.05, greater than 0.1, or greater than 0.15. If z is greater than 0.05, it is easy to maintain the wurtzite structure in a state where the proportion of Sc is high, and the coercive electric field (Ec) is easier to reduce.

[0050] Among them, z is preferably 0.95 or less, and may be 0.9 or less, 0.5 or less, 0.3 or less, or 0.2 or less. In this case, the crystal phase of the aluminum scandium nitride film is likely to be a wurtzite structure.

[0051] In the above formula (B), preferably, x is greater than or equal to 0.3 and less than or equal to 0.7, y is greater than or equal to 0.1 and less than or equal to 0.6, and z is greater than or equal to 0.05 and less than or equal to 0.4. In this case, the coercive electric field is particularly easy to reduce. Furthermore, in the above formula (B), preferably, x is greater than or equal to 0.4 and less than or equal to 0.6, y is greater than or equal to 0.2 and less than or equal to 0.5, and z is greater than or equal to 0.1 and less than or equal to 0.3.

[0052] The thickness of the aluminum scandium nitride film is not particularly limited, and may be less than 10000 nm, less than 2000 nm, less than 1500 nm, less than 1000 nm, less than 500 nm, or less than 250 nm.

[0053] In addition, the aluminum scandium nitride film may have a thickness of 1 nm or more, 2 nm or more, 3 nm or more, 50 nm or more, 100 nm or more, or 175 nm or more.

[0054] In the case where the aluminum scandium nitride film is used in a ferroelectric component, the thickness of the aluminum scandium nitride film is preferably thin. Specifically, the thickness of the aluminum scandium nitride film is preferably less than 250nm. In this case, the ferroelectric component can be used with lower power consumption. The thickness of the aluminum scandium nitride film can be less than 200nm, less than 150nm, less than 100nm, less than 50nm or less than 20nm. Among them, the thickness of the aluminum scandium nitride film can also be more than 1nm, more than 2nm, more than 3nm or more than 5nm.

[0055] In addition, when the aluminum scandium nitride film is used in a piezoelectric component, the thickness of the aluminum scandium nitride film is preferably greater than 250 nm. The thickness of the aluminum scandium nitride film is more preferably greater than 400 nm, and particularly preferably greater than 500 nm. The thickness of the aluminum scandium nitride film may also be less than 10000 nm, less than 5000 nm, or less than 1000 nm.

[0056] <Method for producing aluminum scandium nitride film>

[0057] The aluminum scandium nitride film of the present embodiment can be manufactured by any method as long as it satisfies the above characteristics. For example, the aluminum scandium nitride film of the present embodiment can be obtained by a manufacturing method having the following steps, wherein the step is to form a film by sputtering an aluminum target, a scandium target, and a gallium nitride target. Preferably, the aluminum scandium nitride film of the present embodiment is obtained by a manufacturing method having the following steps, wherein the step is to form a film on a substrate by sputtering an aluminum target, a scandium target, and a gallium nitride target.

[0058] The gallium nitride target includes gallium nitride. Gallium nitride is a bulk whose main component is gallium nitride, and at least one of a single crystal and a polycrystal whose main component is gallium nitride can be listed, and further, a polycrystal whose main component is gallium nitride can be listed. The gallium nitride in the gallium nitride target can also contain indium or aluminum, silicon or the like for exhibiting conductivity or semiconductor properties as a dopant. In addition, in this specification, the so-called "main component" refers to a component with a content of 50% by mass or more.

[0059] The crystal structure of gallium nitride preferably includes a hexagonal structure, and more preferably a hexagonal structure.

[0060] The aluminum target includes aluminum. The aluminum is a bulk whose main component is aluminum, and further, at least one of a single crystal and a polycrystal whose main component is aluminum, and further, a polycrystal whose main component is aluminum. The aluminum in the aluminum target may contain at least one of indium and gallium, or silicon or the like for exhibiting conductivity or semiconductor properties as a dopant.

[0061] The scandium target includes scandium. The scandium is a bulk whose main component is scandium, and further is at least one of a single crystal and a polycrystal whose main component is scandium, and further is a polycrystal whose main component is scandium. The scandium in the scandium target may contain indium or gallium, silicon or the like for exhibiting conductivity or semiconductor properties as a dopant.

[0062] The aluminum target, the scandium target, and the gallium nitride target may each include a backing plate bonded to a bulk body included in each target.

[0063] Each target may further include a bonding material between the bulk and the backing plate. Various materials can be used as the bonding material, but indium is preferred from the viewpoint of suppressing thermal diffusion and thermal expansion during sputtering.

[0064] The substrate used for film formation includes a supporting substrate. The supporting substrate is not particularly limited, and as the supporting substrate, at least one of a silicon substrate and a glass substrate can be exemplified, for example, a silicon substrate, a silicon carbide substrate, a glass substrate including alkali-free glass or quartz, a substrate having a wurtzite structure in a crystal phase such as a gallium nitride substrate, an oxide crystal substrate such as sapphire or magnesium oxide, etc. can be cited. Among them, as the supporting substrate, a silicon substrate is preferably used.

[0065] The substrate may further have an oxide layer on the supporting substrate as required. Examples of oxides constituting the oxide layer include titanium dioxide and silicon dioxide. The oxide layer may be a single layer or a multilayer laminate.

[0066] As a sputtering method, one or more selected from the group consisting of direct current (DC) sputtering, radio frequency (RF) sputtering, alternating current (AC) sputtering, DC magnetron sputtering, RF magnetron sputtering, electron cyclotron resonance (ECR) sputtering, pulsed laser deposition and ion beam sputtering can be appropriately selected. Among these, at least one of DC magnetron sputtering and RF magnetron sputtering is preferred in terms of large-area uniform and high-speed film formation.

[0067] The gas pressure during sputtering is not particularly limited as long as it is 20 mTorr or less. The lower the gas pressure during sputtering, the easier it is for the particles (sputtered particles) released from the target to reach the substrate in a high energy state and to rearrange epitaxially. As a result, a hexagonal aluminum scandium gallium nitride film is easily obtained.

[0068] In addition, the temperature of the substrate during film formation is preferably set to 700° C. or less, and more preferably set to 600° C. or less. In this case, by setting the temperature of the substrate during film formation to 700° C. or less, the film formation time is shortened and the throughput is improved. The temperature of the substrate during film formation only needs to be 150° C. or more or 200° C. or more.

[0069] The gas introduced is not particularly limited as long as it is a gas type that generates sputtering by discharge. As such a gas, at least one of nitrogen and argon can be cited. These can be used alone or in combination. The introduced gas is preferably nitrogen. In this case, the residual polarization tends to become larger.

[0070] The power during discharge can be adjusted appropriately for each target. The power of the target can be adjusted to 0.49W / cm 2 Above and 9.87W / cm 2 The following range can be appropriately adjusted. Thus, by imparting power to the target, coarse target particles are not easily peeled off from the target. If the power during discharge is 2W / cm 2 When the above value is greater than 10%, the plasma is stable and the film forming rate is likely to increase. Furthermore, the value of z in the composition formula (B) can be adjusted by adjusting the power of the gallium nitride target. For example, the greater the power of the target, the greater the value of z.

[0071] The film forming time can be appropriately adjusted according to the thickness of the aluminum scandium nitride film. The longer the film forming time is, the thicker the aluminum scandium nitride film can be.

[0072] <Ferroelectric devices>

[0073] Next, refer to Figure 1The ferroelectric device according to this embodiment will be described. Figure 1 is a cross-sectional view showing a ferroelectric component of this embodiment. Figure 1 As shown, the ferroelectric device 10 includes a first electrode 2 , an aluminum scandium nitride film 3 , and a second electrode 4 in this order on a substrate 1 .

[0074] The ferroelectric component 10 can be driven with low power consumption and can be miniaturized.

[0075] The ferroelectric component 10 can be used, for example, as a storage element such as a ferroelectric memory, or a piezoelectric component such as a pressure sensor or a vibration sensor.

[0076] Example

[0077] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0078] (Example 1)

[0079] A 100 nm thick silicon dioxide (SiO2) film is formed on a supporting substrate including a 5 mm × 5 mm × 600 μm thick crystalline silicon substrate (surface Miller index: (001)). Subsequently, a 50 nm thick titanium dioxide (TiO2) film is formed on the silicon dioxide film. Next, a 100 nm thick platinum (Pt) film (surface Miller index: (111)) is formed on the titanium dioxide film by electron beam evaporation. Thus, a film-forming substrate with a thickness of 0.6 mm is obtained.

[0080] Next, the film-forming substrate obtained in the above manner, the following gallium nitride (GaN) target, the following aluminum (Al) target and the following scandium (Sc) target are installed in a sputtering device, the substrate temperature is set to 400°C, and high-frequency ternary simultaneous reactive magnetron sputtering is performed under the following film-forming conditions, thereby forming an aluminum scandium nitride film on the Pt film of the film-forming substrate, thereby obtaining a layered body having an aluminum scandium nitride film containing Ga (aluminum scandium nitride film / platinum film / titanium dioxide film / silicon dioxide film / silicon substrate).

[0081] (target)

[0082] GaN target

[0083] A target made by bonding GaN polycrystal (sintered body) to a backing plate via an indium bonding material (manufactured by Tosoh Corporation)

[0084] Al target

[0085] A target made by bonding Al polycrystal (sintered body) to a backing plate via an indium bonding material (manufactured by Kojun Chemical Co., Ltd.)

[0086] Sc target

[0087] Target made by bonding Sc polycrystal (sintered body) to a backing plate via an indium bonding material (manufactured by Kojun Chemical Co., Ltd.)

[0088] (film forming conditions)

[0089] Magnetic field strength: 4500 Gauss

[0090] Sc target layer substrate distance: 120mm

[0091] · Distance between Al target layer and substrate: 120mm

[0092] · Distance between GaN target layer and substrate: 120mm

[0093] Sc target power: 4.10W / cm 2 (83W)

[0094] ·Power of Al target: 5.77W / cm 2 (117W)

[0095] GaN target power: 0.99W / cm 2 (20W)

[0096] ·Substrate temperature during film formation: 400°C

[0097] Film forming time: 112 minutes

[0098] Type of introduced gas (sputtering environment): Nitrogen (N2)

[0099] ·Introduction gas flow rate: 75sccm

[0100] Gas pressure during sputtering: 5mTorr

[0101] (Example 2)

[0102] As shown in Table 1, the power of the Sc target (hereinafter sometimes referred to as "target output") was changed to 5.08 W / cm 2 (103W), the output power of the Al target was changed to 4.79W / cm 2 (97W), except for this, a laminate having an aluminum scandium nitride film was obtained in the same manner as in Example 1.

[0103] (Example 3)

[0104] As shown in Table 1, a laminate having an aluminum scandium nitride film was obtained in the same manner as in Example 1 except that the output of the Sc target was changed to 73 W and the output of the Al target was changed to 127 W.

[0105] (Example 4)

[0106] As shown in Table 1, a laminate having an aluminum scandium nitride film was obtained in the same manner as in Example 1 except that the output of the Sc target was changed to 133 W and the output of the Al target was changed to 67 W.

[0107] (Example 5)

[0108] As shown in Table 1, a laminate having an aluminum scandium nitride film was obtained in the same manner as in Example 1 except that the output power of the Sc target was changed to 103 W, the output power of the Al target was changed to 97 W, and the output power of the GaN target was changed to 10 W.

[0109] (Example 6)

[0110] As shown in Table 1, a laminate having an aluminum scandium nitride film was obtained in the same manner as in Example 1 except that the output power of the Sc target was changed to 123 W, the output power of the Al target was changed to 77 W, and the output power of the GaN target was changed to 10 W.

[0111] (Example 7)

[0112] As shown in Table 1, a laminate having an aluminum scandium nitride film was obtained in the same manner as in Example 1 except that the output power of the Sc target was changed to 143 W, the output power of the Al target was changed to 77 W, and the output power of the GaN target was changed to 40 W.

[0113] (Example 8)

[0114] As shown in Table 1, a laminate having an aluminum scandium nitride film was obtained in the same manner as in Example 1 except that the output power of the Sc target was changed to 123 W, the output power of the Al target was changed to 77 W, and the output power of the GaN target was changed to 10 W.

[0115] (Comparative Example 1)

[0116] A laminate having an aluminum scandium nitride film not containing Ga was obtained in the same manner as in Example 1 except that the output of the Sc target was changed to 70 W and the output of the Al target was changed to 130 W as shown in Table 1 without using a GaN target.

[0117] (Comparative Example 2)

[0118] A laminate having an aluminum scandium nitride film not containing Ga was obtained in the same manner as in Example 1 except that the output of the Sc target was changed to 50 W and the output of the Al target was changed to 150 W as shown in Table 1 without using a GaN target.

[0119] (Comparative Example 3)

[0120] A laminate having an aluminum scandium nitride film not containing Ga was obtained in the same manner as in Example 1 except that the output of the Sc target was changed to 60 W and the output of the Al target was changed to 140 W as shown in Table 1 without using a GaN target.

[0121] (Comparative Example 4)

[0122] A laminate having an aluminum scandium nitride film not containing Ga was obtained in the same manner as in Example 1 except that the output of the Sc target was changed to 107 W and the output of the Al target was changed to 93 W as shown in Table 1 without using a GaN target.

[0123] <Evaluation of Aluminum Scandium Nitride Film>

[0124] (1) Determination of crystal structure

[0125] The aluminum scandium nitride films of the laminated bodies of Examples 1 to 8 and Comparative Examples 1 to 4 obtained in the above manner were measured by out-of-plane X-ray diffraction profile measurement and in-plane X-ray diffraction profile measurement to determine the type of crystal structure, the lattice constant a of the a-axis of the unit lattice, and the X-ray diffraction profile of the laminated bodies. Lattice constant of c-axis c / a and internal parameter u were investigated. Furthermore, the Out-of-Plane method is a method for evaluating the lattice plane parallel to the surface of the sample, and the X'pert MRD (manufactured by PANalytical) was used to perform θ-2θ scanning and X-ray diffraction measurement. In addition, the In-Plane method is a method for evaluating the lattice plane perpendicular to the surface of the sample, and the X-ray diffraction measurement was performed using Smart Lab (manufactured by Rigaku).

[0126] As a result, for Examples 1 to 8 and Comparative Examples 1 to 4, diffraction peaks (002) and (004) were observed in the X-ray diffraction profiles obtained by the out-of-plane method, and thus it was found that the aluminum scandium nitride film had a wurtzite-type crystal phase. In addition, in the aluminum scandium nitride film of Example 1, the lattice constant of the a-axis is The lattice constant of the c-axis is The internal parameter u is 0.385. In addition, for the aluminum scandium nitride films of Examples 2 to 8 and Comparative Examples 1 to 4, the internal parameter u is shown in Table 1. The X-ray diffraction profiles obtained by the out-of-plane method and the X-ray diffraction profiles obtained by the in-plane method of Example 1 are shown in Tables 1 and 2, respectively. Figure 2 and Figure 3 middle.

[0127] (2) Determination of crystal phase composition and film thickness

[0128] The composition and film thickness of the aluminum scandium nitride films of the laminates of Examples 1 to 8 and Comparative Examples 1 to 4 were determined using a wavelength dispersive X-ray fluorescence analyzer (product name: PW4400, manufactured by PANalytical).

[0129] (3) Evaluation of ferroelectricity

[0130] On the aluminum scandium nitride films of the laminates of Examples 1 to 8 and Comparative Examples 1 to 4 obtained as described above, platinum (Pt) electrodes having a diameter of 50 μm and a thickness of 75±25 nm were formed at room temperature by electron beam deposition to prepare samples.

[0131] For this sample, the ferroelectricity was evaluated using a ferroelectric tester (product name: "FCE-1A", manufactured by Dongyang Technology Co., Ltd.). Specifically, at room temperature, an electric field E was applied (measurement frequency: 10 kHz) and a PE measurement was performed to measure the polarization P relative to the electric field E, and the residual polarization Pr and the coercive electric field Ec after 5 cycles were obtained. The results are shown in Table 1. Furthermore, in Table 1, with respect to the residual polarization Pr, the absolute value of the maximum residual polarization Pr observed in the PE measurement is shown. In addition, with respect to the coercive electric field Ec, the absolute value of the electric field at the intersection of the hysteresis curve obtained by the PE measurement and P=0 is shown.

[0132] (4) Evaluation of piezoelectric properties

[0133] On the aluminum scandium nitride films of the laminates of Examples 7 to 8 and Comparative Example 4 obtained as described above, platinum (Pt) electrodes having a diameter of 50 μm and a thickness of 75±25 nm were formed at room temperature by electron beam evaporation to prepare samples.

[0134] For this sample, use d 33 The piezoelectric constant d was measured at room temperature using a piezoelectric constant analyzer (product name: "PM300", manufactured by Piezo Test, Ltd.). 33 The piezoelectric characteristics were evaluated. The results are shown in Table 1.

[0135] [Table 1]

[0136]

[0137] It can be seen that the PE curves of the aluminum scandium nitride films of Examples 1 to 8 and Comparative Examples 1 to 4 all draw hysteresis loops. Therefore, it was confirmed that the aluminum scandium nitride films of Examples 1 to 8 and Comparative Examples 1 to 4 all have ferroelectricity.

[0138] In addition, according to the results shown in Table 1, the coercive electric field Ec of Examples 1 to 8 showed a value lower than the coercive electric field Ec of Comparative Examples 1 to 4.

[0139] It was confirmed that the aluminum scandium nitride films of Examples 1 to 8 can reduce the coercive electric field Ec and increase the remanent polarization Pr, compared with the aluminum scandium nitride films of Comparative Examples 1 to 4.

[0140] In addition, according to the results shown in Table 1, the piezoelectric constants d of the aluminum scandium nitride films of Examples 7 and 8 are 33 The absolute value of is greater than the piezoelectric constant d of the aluminum scandium nitride film of Comparative Example 4. 33 Therefore, it can be seen that the ferroelectric component of the present invention can also be used in a piezoelectric component.

[0141] Description of Reference Numerals

[0142] 1 substrate, 2 first electrode, 3 scandium aluminum nitride film, 4 second electrode, 10 ferroelectric component.

Claims

1. An aluminum scandium nitride film comprising aluminum, scandium and nitrogen, and further comprising gallium.

2. The aluminum scandium nitride film according to claim 1, wherein: The crystalline phase of the aluminum scandium nitride film includes hexagonal crystals.

3. The aluminum scandium nitride film according to claim 2, wherein: The crystal phase is a wurtzite structure.

4. The aluminum scandium nitride film according to claim 3, wherein: The internal parameter u defined by the following formula (A) is less than 1.0, Internal parameter u=(a 2 / 3c 2 )+0.25(A) In the above formula (A), a represents the lattice constant of the a-axis. c represents the lattice constant of the c-axis 5. The aluminum scandium nitride film according to claim 4, wherein: The internal parameter u is greater than or equal to 0.30 and less than or equal to 0.

50.

6. The aluminum scandium nitride film according to claim 1, wherein: The aluminum scandium nitride film is represented by the following composition formula (B): (Al x Sc y Ga z )N(B) In the above formula (B), x is 0.4 to 0.6, y is 0.1 to 0.5, z is 0.1 to 0.3, and x+y+z is 1. 7 . The aluminum scandium nitride film according to claim 1 , having a thickness of 2000 nm or less. The aluminum scandium nitride film according to claim 7 , which has a thickness of 250 nm or less.

9. The aluminum scandium nitride film according to claim 1, wherein the thickness thereof is greater than 250 nm. 10 . A ferroelectric device comprising the aluminum scandium nitride film according to claim 1 .