Non-woven fabric using hyaluronate fibers and method for producing same

By adjusting the moisture content and drying conditions of the hyaluronate paste, a rough surface hyaluronate fiber is formed, and a non-woven fabric is made by needle-punching, the hyaluronate nanofibers in the prior art are solved by fragile physical properties and low productivity of hyaluronate nanofibers in the prior art. The problem of this paper realizes the preparation of high-strength non-woven fabrics and is suitable for applications of a variety of biological materials.

CN118974336AActive Publication Date: 2024-11-15JINWOO BIO
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202280094094.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-23
Filing Date
2022-05-31
Publication Date
2024-11-15
Estimated Expiration
2042-05-31

AI Technical Summary

Technical Problem

The existing hyaluronic acid nanofiber manufacturing methods require the use of volatile solvents, which leads to fragile physical properties and low productivity, making it difficult to achieve high-strength non-woven fabric productization and commercialization.

Method used

By producing a hyaluronate paste with a moisture content of 50-95%, the nozzle is extruded and dried after melting to form hyaluronate fibers with rough surfaces, and hyaluronate with excellent adhesion and tensile strength is produced by needle puncture. Acid non-woven fabric.

Benefits of technology

The mass manufacturing of high-strength hyaluronate fibers has been achieved, and non-woven fabrics with excellent adhesion and tensile strength are prepared, suitable for skin external agent patches and tissue repair biological materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974336A_ABST
    Figure CN118974336A_ABST
Patent Text Reader

Abstract

The present invention relates to a hyaluronate non-woven fabric using hyaluronate fibers and a method for manufacturing the same, and more particularly, to a highly functional hyaluronate non-woven fabric manufactured from hyaluronate fibers having rough surfaces and small diameters, and a method for manufacturing the same. A method for producing a hyaluronate nonwoven fabric according to the present invention is characterized by comprising: (a) a step for producing hyaluronate fibers; (b) a step in which the produced hyaluronate fiber is subjected to a curl treatment; (c) a step for cutting the hyaluronate fiber to which the curl has been imparted; (d) forming a web using the cut hyaluronate fibers; and (e) a step for needling the formed hyaluronate web. The hyaluronate non-woven fabric according to the present invention contains high-concentration hyaluronate, is manufactured by needling high-strength hyaluronate fibers, has excellent adhesion and tensile strength, and can be used in various fields such as skin external application patches, tissue repair biomaterials, anti-adhesion covering materials, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a hyaluronate nonwoven fabric using hyaluronate fibers and a method for manufacturing the same, and more particularly, to a highly functional hyaluronate nonwoven fabric made of hyaluronate fibers having a rough surface and a micro-diameter and a method for manufacturing the same. Background Art

[0002] Nonwoven fabrics are fiber structures with a planar structure that are made by combining various fibers such as natural fibers, chemical fibers, glass fibers, and metal fibers into a tangled web based on their properties and mechanically or physically bonding them. Nonwoven fabrics are widely used in various industrial fields based on their uses, properties, and functions. Furthermore, research is being conducted on various nonwoven fabrics by mixing components that can give nonwoven fabrics secondary processing or various functionalities.

[0003] Recently, the consumption of products using nonwoven fabrics has been increasing in many industrial fields. For example, nonwoven fabrics are pressed at high temperatures to produce hard panels, which are used as automotive facing materials or building facing materials. In a wide range of fields such as clothing, hygiene, civil engineering, construction, automobiles, and medical care, research is being focused on high-value-added nonwoven fabric products that have high functional effects, rather than simple product uses. In particular, nonwoven fabric products used in the medical market are used not only as surgical gowns, masks, and other wearable products, but also as surgical sheets, pads, dressings, and filter materials, and as tissue supports inserted for internal organ regeneration.

[0004] In order to manufacture such medical nonwoven fabrics, various biodegradable polymers are used. Biodegradable polymers are a general term for polymers that gradually lose their shape and weight while slowly undergoing chemical degradation in the body. Representative natural polymers include collagen, fibronectin, gelatin, chitosan, and alginic acid. Synthetic polymers include polylactic acid (PLA), polyglycolic acid (PGA), polylactic-co-glycolic acid (PLGA) and similar copolymers, polycaprolactone (PCL), polyanhydrides, and polyorthoesters.

[0005] Korean Patent No. 1329261 discloses a functional nonwoven fabric using chitosan and a method for manufacturing the same, and Korean Patent No. 2002586 discloses a thermally bonded nonwoven fabric including natural fibers uniformly coated with chitosan on cellulose fibers.

[0006] On the other hand, hyaluronic acid (HA), a mucopolysaccharide existing in the dermis, is a disaccharide composed of N-acetylglucosamine and D-glucuronic acid via a β-1,4-glucosidic bond, and is a biopolymer substance linked via a β-1,3-glucosidic bond to form a hyaluronate chain.

[0007] Hyaluronic acid is evenly distributed in the connective tissue, epithelium and nerve tissue of the human body. As a biocompatible material with various physiological activities, its effects on skin regeneration and moisturizing, maintaining elasticity and improving wrinkles have been proven. Therefore, recently, the industry has required the manufacture of non-woven fabrics in order to use this hyaluronic acid fiber for wound dressings, cosmetic patches, anti-adhesion coatings, etc. The hyaluronic acid fiber used as the raw material of the non-woven fabric has the following problems depending on its manufacturing method.

[0008] The method for manufacturing hyaluronic acid nanofibers requires a step for further removing volatile organic solvents such as DMF, DMSO, formic acid, etc. that must be used in the manufacture of nanofibers. When manufacturing nonwoven fabrics, nanofiber nonwoven fabrics are inconvenient to use alone and have the disadvantage of being physically fragile. In addition, the productivity per unit time is very low, resulting in a problem of high production unit price.

[0009] In order to solve this problem, Korean Patent No. 2338355 discloses a wet non-woven fabric manufacturing method, but the physical properties are also fragile and the manufacturing process is slightly complicated, so a more efficient manufacturing method needs to be studied. When used as a non-woven fabric, if the physical properties above the established strength cannot be achieved, the processing operations such as cutting required for productization cannot be performed, making it difficult to achieve commercialization.

[0010] Therefore, the present inventors have devoted themselves to solving the above-mentioned problems and have found that by manufacturing a hyaluronate paste with a moisture content of 50 to 95% by weight, extruding it through a nozzle after melting and drying it, a large amount of hyaluronate fibers with a rough surface and excellent tensile strength can be manufactured, and by using it for needle punching, a hyaluronate non-woven fabric with excellent adhesion and tensile strength can be manufactured, thereby completing the present invention. Summary of the invention

[0011] Technical issues

[0012] The object of the present invention is to provide a hyaluronate nonwoven fabric and a method for producing the same, which not only can adhere to the skin or the body when used, but also has excellent mechanical properties required for processing, and can be effectively used as a skin external agent patch, a tissue repair biomaterial, or an anti-adhesion covering material, etc.

[0013] Technical Solution

[0014] In order to achieve the above-mentioned object, the present invention provides a hyaluronate nonwoven fabric comprising hyaluronate fibers, characterized in that, when measured by the following measuring method, the bending angle is 2 to 10°, the moisture content is 5 to 25% by weight, and the hyaluronate content is 90% by weight or more relative to the total weight of the fibers excluding moisture.

[0015] <Bending angle measurement method>

[0016] (a) Prepare HA fibers with a length of 20 cm and a diameter of 1 mm.

[0017] (b) Fix one end of the HA fiber 3cm above the plate

[0018] (c) Using the extended line (B) of the upper side of the plate as a reference, measure the angle (θ) formed by the extended line (T) of the other end of the HA fiber.

[0019] In the present invention, it is characterized in that the tensile strength of the hyaluronate fiber is 3 to 15 kg / mm 2 .

[0020] In the present invention, it is characterized in that the adhesive force of the hyaluronate nonwoven fabric is 0.9 to 2.7 kPa.

[0021] In the present invention, it is characterized in that the thickness of the hyaluronate nonwoven fabric is 1 to 10 mm.

[0022] In the present invention, it is characterized in that the tensile strength of the hyaluronate nonwoven fabric is 0.3 to 1.5 kg / mm 2 .

[0023] In the present invention, it is characterized in that the hyaluronate nonwoven fabric is used as a skin external application patch, a tissue repair biomaterial or an anti-adhesion covering material.

[0024] The present invention provides a method for producing a hyaluronate nonwoven fabric, which is characterized by comprising: (a) a step of producing hyaluronate fibers; (b) a step of curling the produced hyaluronate fibers; (c) a step of cutting the curled hyaluronate fibers; (d) a step of forming a net using the cut hyaluronate fibers; and (e) a step of needle-punching the formed hyaluronate net.

[0025] In the present invention, it is characterized in that the step of manufacturing hyaluronate fibers comprises: (a-1) adjusting the water content of hyaluronate having a weight average molecular weight of 100 to 3,000 kDa to 50 to 95 weight % to manufacture a hyaluronate paste; (a-2) melting the hyaluronate paste having the adjusted water content at 15 to 100° C. and extruding it through a nozzle; and (a-3) drying the extruded spinning fluid to form fibers.

[0026] In the present invention, it is characterized in that when forming the net, fibers made of a polymer material selected from the group consisting of collagen, fibronectin, gelatin, chitosan, alginate, polylactic acid (PLA), polyglycolic acid (PGA), polylactic acid-glycolic acid copolymer (PLGA) and polycaprolactone (PCL) are mixed.

[0027] Effects of the Invention

[0028] The hyaluronate nonwoven fabric of the present invention contains high-concentration hyaluronate and is produced by needle-punching high-strength hyaluronate fibers, and has excellent adhesive force and tensile strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a photograph for evaluating the roughness of hyaluronate fibers of one embodiment of the present invention. (A: smooth hyaluronate fibers, B: rough hyaluronate fibers)

[0030] Figure 2 It is an explanatory diagram of a method for measuring the bending angle of hyaluronate fibers according to one embodiment of the present invention.

[0031] Figure 3 This is a photograph of a hyaluronate fiber according to an embodiment of the present invention. (A: hyaluronate fiber, B: hyaluronate fiber with curl)

[0032] Figure 4 This is a photograph of a hyaluronate nonwoven fabric produced by a needle punching method according to an embodiment of the present invention.

[0033] Figure 5 This is a photo of a hyaluronate and chitosan mixed nonwoven fabric according to an embodiment of the present invention.

[0034] Figure 6 This is a microstructure photograph of the needle-punched nonwoven fabric of the present invention. (A: hyaluronate nonwoven fabric, B: hyaluronate and chitosan mixed nonwoven fabric) DETAILED DESCRIPTION

[0035] Best Mode for Carrying Out the Invention

[0036] In the present invention, it is to be confirmed that when a hyaluronate paste having a moisture content adjusted to a specific range is spun through a nozzle at a predetermined temperature and dried at a high temperature but not at a normal temperature, hyaluronate fibers having a very rough fiber surface can be produced, and when the hyaluronate paste is needle-punched, a nonwoven fabric having excellent adhesion and mechanical strength can be produced.

[0037] In the present invention, the water content of hyaluronate is adjusted to 50 to 95% by weight to prepare a paste, the hyaluronate paste is melted at 15 to 100° C. and then extruded through a nozzle, and then dried at 100 to 150° C. to produce a large amount of hyaluronate paste having a water content of 5 to 25% by weight and a tensile strength of 3 to 15 kg / mm 2 , hyaluronate fibers with very rough surfaces. After applying heat to the manufactured hyaluronate fibers to give curls, they are cut to a predetermined length, formed into a web by carding and air-laying processes, and then needle-punched, and the formed nonwoven fabric is pressed to manufacture a nonwoven fabric with excellent adhesion and tensile strength.

[0038] Therefore, the present invention relates to a method for producing a hyaluronate nonwoven fabric, which is characterized in that it includes: (a) a step of producing hyaluronate fibers; (b) a step of curling the produced hyaluronate fibers; (c) a step of cutting the curled hyaluronate fibers; (d) a step of forming a net using the cut hyaluronate fibers; and (e) a step of needle-punching the formed hyaluronate net.

[0039] In the present invention, the steps of manufacturing hyaluronate fibers include: (a-1) adjusting the moisture content of hyaluronate having a weight average molecular weight of 100 to 3,000 kDa to 50 to 95 weight % to manufacture a hyaluronate paste; (a-2) melting the hyaluronate paste having the adjusted moisture content at 15 to 100° C. and extruding it through a nozzle; and (a-3) drying the extruded spinning fluid to form fibers.

[0040] In the present invention, hyaluronate is a substance in which a salt is bonded to hyaluronic acid, and examples thereof include sodium hyaluronate, calcium hyaluronate, potassium hyaluronate, etc., but are not limited thereto.

[0041] In the present invention, the molecular weight of the hyaluronate is preferably 100 to 3,000 kDa. In addition, the hyaluronate paste has a water content of 50 to 95% by weight.

[0042] The hyaluronate paste can be prepared by adding a solvent to hyaluronate. Preferably, water or an ethanol solution is used as the solvent, and the mixture is mixed until the solvent is uniformly mixed.

[0043] In order to smoothly carry out the mass spinning process, the moisture content of the hyaluronate paste can be 50 to 95% by weight, preferably 88 to 92% by weight. When the moisture content is less than 50% by weight, high pressure is required during spinning. When the moisture content exceeds 95% by weight, it is in a liquid form compared to the paste, so there is a problem of broken fibers during spinning.

[0044] In the present invention, it is characterized in that after manufacturing the hyaluronate paste, a step of placing it at 0 to 100° C. for 6 to 12 hours is performed to achieve water balance. When the temperature range and time range are exceeded, water balance cannot be achieved normally. The water balance is used to make the water molecules of the paste and the hyaluronic acid uniformly mixed. When spinning is performed without water balance, the water molecules and the hyaluronic acid are not uniformly mixed, so that the spinning cannot be performed at a predetermined speed during spinning.

[0045] In the present invention, a hyaluronate paste having a water content of 50 to 95% by weight is added to a spinning device, melted at 15 to 100° C., and extruded through a nozzle to produce a spinning fluid. At this time, when the temperature is lower than 15° C., the hyaluronate paste does not melt and cannot be extruded, and when the temperature exceeds 100° C., there is a problem of boiling of the paste.

[0046] In the present invention, the extruded spinning fluid is dried to finally form fibers, and the drying is preferably carried out at 100 to 150° C. depending on the moisture content of the paste. When the drying temperature is lower than 100° C., the surface of the manufactured fiber is smooth, so that the entanglement force is weak during the needle punching process after forming a web, and it is difficult to form a nonwoven fabric. When the drying temperature exceeds 150° C., there are problems of fiber browning and cracking.

[0047] The hyaluronate content of the produced hyaluronate fiber can be made to be 90% by weight or more, the water content is 5 to 25% by weight, and the tensile strength is 3 to 15 kg / mm 2 The surface is very rough, so when it is used to make non-woven fabrics, non-woven fabrics with various densities and physical properties can be produced.

[0048] The method for producing the hyaluronate nonwoven fabric of the present invention is characterized in that the hyaluronate fibers are curled by heat treatment to increase the intersecting force between the fibers. During the heat treatment, the hyaluronate fibers are subjected to hot air treatment at a high temperature of 70° C. or higher to impart curls.

[0049] In order to form a web for making a nonwoven fabric, the obtained hyaluronate fibers can be cut into a desired length and formed into a web by a carding and air-laying process, that is, the cut hyaluronate fibers are dispersed by air pressure and then ejected by air pressure.

[0050] The needling step of the present invention is a step of needling the flat sheet web formed above. Specifically, the needling step is to repeatedly move a needle plate with needles up and down while passing through a needle loom, so that a part of the two-dimensional random fiber arrangement is combined into a three-dimensional random structure to produce a non-woven fabric.

[0051] The method for producing the hyaluronate nonwoven fabric of the present invention can be mixed with fibers made of biocompatible materials when forming the net. That is, in order to ensure more diverse physical properties and functionality, collagen, fibronectin, gelatin, chitosan, alginic acid, polylactic acid (PLA), polyglycolic acid (PGA), polylactic-co-glycolic acid (PLGA), polycaprolactone (PCL), etc., which are pharmacologically acceptable biocompatible materials and can be used to produce fibers, can be mixed with hyaluronic acid fibers.

[0052] Another aspect of the present invention relates to a hyaluronate nonwoven fabric comprising hyaluronate fibers, characterized in that, when measured by the following measurement method, the bending angle is 2 to 10°, the moisture content is 5 to 25% by weight, and the hyaluronate content is greater than 90% by weight relative to the total weight of the fibers excluding moisture.

[0053] <Bending angle measurement method>

[0054] (a) Prepare HA fibers with a length of 20 cm and a diameter of 1 mm.

[0055] (b) Fix one end of the HA fiber 3cm above the plate

[0056] (c) Using the extension line (B) of the upper side of the plate as a reference, measure the angle (θ) formed by the extension line (T) of the other end of the HA fiber.

[0057] The tensile strength of the hyaluronate fiber is 3 to 15 kg / mm 2 , so it can be used to make nonwoven fabrics by needle punching. The tensile strength of hyaluronate fiber is less than 3kg / mm 2 When the fiber breaks, it is difficult to process. When the fiber exceeds 15kg / mm 2 When it is made into non-woven fabric, the material is stiff and may cause inconvenience in use.

[0058] The hyaluronate nonwoven fabric of the present invention preferably has a thickness of 1 to 10 mm. The obtained nonwoven fabric is characterized in that, depending on the thickness of the nonwoven fabric, it has a density of 0.3 to 1.5 kg / mm. 2 The tensile strength and adhesion are 0.9~2.7kPa.

[0059] The hyaluronate nonwoven fabric of the present invention has excellent adhesive force and tensile strength, and can be used as a skin external preparation patch, a tissue repair biomaterial, an anti-adhesion covering material, and the like.

[0060] Specific ways to implement the invention

[0061] The present invention will be described in more detail below by way of examples. These examples are only used to illustrate the present invention and should not be interpreted as limiting the scope of the present invention by these examples, which is self-evident to those skilled in the art.

[0062] Example 1: Preparation of hyaluronate paste

[0063] Sodium hyaluronate (Hi-Aqua TM , Zhenyu Biological Co., Ltd.) was added with water, mixed and stirred to produce a hyaluronate paste having a water content of 50 to 95% by weight. The prepared hyaluronate paste was refrigerated and stored at 4° C. for 12 hours to promote water balance.

[0064] Example 2: Production of hyaluronate fibers by spinning

[0065] The hyaluronate paste prepared in Example 1 was placed in the storage part of the spinning device, melted at 15 to 100° C., pressurized, spun through a nozzle, and dried at 120° C. to produce hyaluronate fibers with a moisture content of 5 to 25% by weight.

[0066] Comparative Example 1: Production of hyaluronate fibers by spinning

[0067] The hyaluronate paste prepared in Example 1 was placed in a storage portion of a spinning device, melted at 15 to 100° C., pressurized, spun through a nozzle, and dried at 50° C. to produce hyaluronate fibers having a moisture content of 5 to 25% by weight.

[0068] Comparative Example 2: Production of hyaluronate fibers by spinning

[0069] The hyaluronate paste prepared in Example 1 was placed in a storage portion of a spinning device, melted at 15 to 100° C., pressed, and spun through a nozzle, and dried at 160° C. to produce hyaluronate fibers.

[0070] Experimental Example 1: Evaluation of the fiber roughness of hyaluronate fibers at different drying temperatures

[0071] The surface roughness of the fibers obtained in Example 2, Comparative Example 1 and Comparative Example 2 was evaluated using a microscope. Figure 1 ).

[0072] As a result, fibers with a moisture content of 5 to 25% by weight were spun under drying conditions of 50°C (Comparative Example 1) and 120°C (Example 2), and it was confirmed that the surface of the fibers dried at 50°C was spun in a smooth form, while the surface of the fibers dried at 120°C was spun in a rough form. The moisture content of Comparative Example 2, in which the drying temperature was 160°C, was 1 to 5% by weight, and the fibers were browned and cracks were excessively formed.

[0073] Experimental Example 2: Measurement of the bending angle of hyaluronate fibers

[0074] The bending angle of the hyaluronate fiber obtained in Example 2 was measured as follows (refer to Figure 2 ) and the results are shown in Table 1.

[0075] (a) Prepare HA fibers with a length of 20 cm and a diameter of 1 mm.

[0076] (b) Fix one end of the HA fiber 3cm above the plate

[0077] (c) Using the extension line (B) of the upper side of the plate as a reference, measure the angle (θ) formed by the extension line (T) of the other end of the HA fiber.

[0078]

Table 1

[0079]

[0080]

[0081] From Table 1 above, it can be seen that when the moisture content of hyaluronate fiber exceeds 25% by weight, the bending angle exceeds 10°, making it difficult to form a net or manufacture non-woven fabrics by needle punching. Even if it is manufactured into non-woven fabrics, it will be impossible to carry out processing operations such as cutting required for productization due to the reduction in physical properties, which will cause problems in commercialization.

[0082] It was also confirmed that when the water content of the hyaluronate fiber was less than 5% by weight, the fiber shape was maintained but the shape was rigid and lacked flexibility, and thus the fiber was easily broken.

[0083] On the contrary, it was found that when the moisture content of the hyaluronate fibers was 5 to 25% by weight, the bending angle was 2 to 10°, and the hyaluronate fibers were in a form suitable for needle punching to produce nonwoven fabrics.

[0084] Experimental Example 3: Measurement of the tensile strength of hyaluronate fibers

[0085] The tensile strength of the hyaluronate fiber obtained in Example 2 was measured and the results are shown in Table 2. A sample having a length of 5 cm was attached to a test fixture and the tensile strength was measured using a universal material testing machine at a crosshead speed of 2 mm / min.

[0086]

Table 2

[0087] Hyaluronate fiber moisture content (weight %) <![CDATA[Tensile strength (kg / mm 2 )]]> 50 0.27 30 2.83 25 3.24 20 5.29 10 10.53 5 13.38

[0088] From Table 2 above, it can be seen that when the moisture content of hyaluronate fiber is above 50 wt %, the tensile strength drops sharply, it is easy to break, and it has no elasticity, so it cannot perform the function of fiber normally.

[0089] When the moisture content of the hyaluronate fiber is 5% by weight or less, the fiber shape is maintained but the shape is rigid and easily broken, so that the tensile strength cannot be measured.

[0090] On the contrary, it is known that when the moisture content of hyaluronate fiber is 5 to 25 wt%, the tensile strength is 3.24 to 13.38 kg / mm 2 , so that hyaluronate fibers can exert the morphology and function of silk.

[0091] Example 3: Production of hyaluronate nonwoven fabric by needle punching

[0092] 1) Production of hyaluronate fibers

[0093] By the method of Example 2, hyaluronate fibers (tensile strength: 3 to 15 kg / mm) having a bending angle of 2 to 10°, a moisture content of 5 to 25% by weight, and a hyaluronate content of 90% by weight or more relative to the total weight of the fiber excluding moisture were produced. 2 )( Figure 3 A).

[0094] 2) Curl treatment

[0095] The obtained hyaluronate fibers were subjected to hot air treatment at 70 to 100° C. to produce hyaluronate fibers ( Figure 3 B).

[0096] 3) Cutting

[0097] The curled hyaluronate fibers were cut into a predetermined length of 3 to 7 cm using a cutter.

[0098] 4) Forming a web by carding and air-laying

[0099] The cut hyaluronate fibers were dispersed by air pressure and then ejected by air pressure to form a web.

[0100] 5) Acupuncture

[0101] The multi-layer sheet formed into a net was needle punched to produce a uniform nonwoven fabric (average thickness 5 mm) ( Figure 4 ).

[0102] Comparative Example 3: Production of hyaluronate nonwoven fabric by needle punching

[0103] By using the method of Comparative Example 1, hyaluronate fibers (tensile strength: 3 to 15 kg / mm) having a bending angle of 2 to 10°, a moisture content of 5 to 25% by weight, and a hyaluronate content of 90% by weight or more relative to the total weight of the fiber excluding moisture were produced. 2 ), and a hyaluronate nonwoven fabric was prepared by the same method as in Example 3.

[0104] As a result, it was confirmed that when using hyaluronate fibers with a smooth surface, the fiber entanglement force was weak during the needle punching process after forming a web, and a nonwoven fabric could not be formed satisfactorily.

[0105] Example 4: Production of nonwoven fabrics mixed with hyaluronate and chitosan by needle punching

[0106] 1) Production of hyaluronate fibers

[0107] By using the method of Example 2, hyaluronate fibers (tensile strength: 3 to 15 kg / mm) having a bending angle of 2 to 10°, a moisture content of 5 to 25% by weight, and a hyaluronate content of 90% by weight or more relative to the total weight of the fiber excluding moisture were produced. 2 ).

[0108] 2) Chitosan fiber

[0109] Manufacturer: Saturn Biotech, diameter 0.006~0.018mm

[0110] 3) Curl treatment

[0111] The obtained hyaluronate fibers were subjected to hot air treatment at a high temperature of 70 to 100° C. to produce hyaluronate fibers imparted with curl.

[0112] Chitosan fibers with curls are produced by heat-treating chitosan fibers with steam at 100° C. or higher or by the same heat-treatment process as hyaluronate.

[0113] 4) Cutting

[0114] The curled hyaluronate and chitosan fibers were cut into a predetermined length of 3 to 7 cm using a cutter.

[0115] 5) Forming a web by carding and air-laying and needle punching

[0116] The cut hyaluronate fibers and chitosan fibers were mixed at a ratio of 50:50 wt %, and processed in the same manner as in Example 3 to produce a nonwoven fabric (average thickness 5 mm) mixed with hyaluronate and chitosan. Figure 5 ).

[0117] Experimental Example 4: Confirmation of the microstructure of nonwoven fabric

[0118] The microstructure of the hyaluronate nonwoven fabrics prepared in Examples 3 and 4 was confirmed using a microscope (CX33RTFS2, Olympus Corporation, Korea). Figure 6 ). It was confirmed that the nonwoven fabric structure had a net-like structure in which the fibers were cross-linked, and in particular, the nonwoven fabric mixed with chitosan confirmed that the hyaluronate fibers and the chitosan fibers were well mixed. Compared with nonwoven fabrics produced by wet spinning, the net-like nonwoven fabric had spaces between the cross-links between the fibers, had better physical properties, and was easy to process and use.

[0119] Experimental Example 5: Measurement of the gelation degree of hyaluronate nonwoven fabric

[0120] The gelation degree of a pure hyaluronate nonwoven fabric produced by needle punching (Example 3) and a nonwoven fabric containing 50% by weight of hyaluronate and chitosan (Example 4) were measured as shown below.

[0121] A 2×2 cm pure hyaluronate nonwoven fabric and a nonwoven fabric containing 50% hyaluronate and chitosan were immersed in purified water for 5 seconds and then taken out. The weight was measured after removing the external moisture of the nonwoven fabric, and the gelation degree was measured. The gelation degree was calculated as follows.

[0122] Degree of gelation (%) = (weight after gelation - weight before gelation / weight before gelation) × 100

[0123]

Table 3

[0124]

[0125] It can be seen that the solubility of the nonwoven fabric containing chitosan in water is very low, and the degree of gelation is lower than that of the pure hyaluronate nonwoven fabric.

[0126] Experimental Example 6: Testing the Adhesion of Hyaluronate Nonwoven Fabric

[0127] Using a texture analyzer (TA) (QM100SN, Qmesys, Korea), the adhesion of a pure hyaluronate nonwoven fabric produced by needle punching (Example 3, pure hyaluronate nonwoven fabric with a moisture content of 25 wt%) and a nonwoven fabric containing 50% hyaluronate and 50% chitosan respectively (Example 4, hyaluronate + chitosan nonwoven fabric with a moisture content of 25 wt%, 50:50 wt% ratio) was measured as follows.

[0128] The pig skin was cut into 3×3 cm rectangles and placed in room temperature water for 24 hours. After the moisture content was adjusted to 22.3%, it was attached to the upper and lower probes of the texture analyzer. Then, 2×2 cm rectangles of pure hyaluronate non-woven fabric, non-woven fabric mixed with chitosan, and non-woven fabric composed only of chitosan were placed on the pig skin below and pressed at a pressure of 3.2 kPa for 3 minutes, and then peeled off at a speed of 10 mm / min and the adhesion was measured.

[0129]

Table 4

[0130] sample Adhesion (kPa) Pure hyaluronate nonwoven fabric 2.7 Hyaluronate + Chitosan Non-woven Fabric 0.9 Chitosan nonwoven fabric 0

[0131] It was confirmed that the nonwoven fabric composed of pure chitosan alone had no adhesive strength. It was found that the nonwoven fabric composed of pure hyaluronate had higher adhesive strength than the nonwoven fabric mixed with chitosan because the degree of gelation was high and the adhesive strength was increased.

[0132] It was also found that the nonwoven fabric mixed with chitosan also exhibited a certain adhesive force.

[0133] This shows that nonwoven fabrics with high physical properties can be produced by mixing appropriate amounts of hyaluronate and chitosan, producing nonwoven fabrics, adjusting the degree of gelation, and imparting targeting ability by regulating the in vivo persistence and imparting adhesion.

[0134] Experimental Example 7: Measurement of the tensile strength of hyaluronate nonwoven fabric

[0135] The tensile strength of pure hyaluronate nonwoven fabric produced by needle punching (Example 3, pure hyaluronate nonwoven fabric with a moisture content of 25% by weight) and nonwoven fabric containing 50% of hyaluronate and 50% of chitosan (Example 4, hyaluronate + chitosan nonwoven fabric with a moisture content of 25% by weight, 50:50% by weight ratio) was measured and the results are shown in Table 5. A sample with a length of 5 cm was attached to a test fixture, and the tensile strength was measured using a universal material testing machine at a crosshead speed of 2 mm / min.

[0136]

Table 5

[0137] sample Tensile strength(kgf) Pure hyaluronate nonwoven fabric 0.3 Hyaluronate + Chitosan Non-woven Fabric 1.5

[0138] It can be seen from Table 5 that when chitosan fibers are mixed with pure hyaluronate fibers, higher tensile strength is exhibited. It can be seen that when chitosan fibers are mixed when forming nonwoven fabrics, the chitosan fibers are entangled between the hyaluronate nonwoven fabrics to exhibit stronger bonding force.

[0139] The above detailed description of the specific parts of the present invention is only a preferred embodiment, and is not intended to limit the scope of the present invention, which is self-evident to those skilled in the art. Therefore, the substantive scope of the present invention is defined by the attached claims and their equivalents.

[0140] Industrial Applicability

[0141] The hyaluronate nonwoven fabric of the present invention has excellent adhesive force and tensile strength, and can be used in various fields such as skin external preparation patches, tissue repair biomaterials, and anti-adhesion covering materials.

Claims

1. A hyaluronate nonwoven fabric comprising hyaluronate fibers, It is characterized in that When measured by the following measurement method, the bending angle is 2 to 10°, the moisture content is 5 to 25% by weight, and the hyaluronate content is 90% by weight or more relative to the total weight of the fiber excluding moisture. <Bending Angle Measurement Method> (a) Prepare HA fibers with a length of 20 cm and a diameter of 1 mm. (b) Fix one end of the HA fiber 3cm above the plate (c) Using the extended line (B) of the upper side of the plate as a reference, measure the angle (θ) formed by the extended line (T) of the other end of the HA fiber.

2. The hyaluronate nonwoven fabric according to claim 1, It is characterized in that The tensile strength of the hyaluronate fiber is 3 to 15 kg / mm 2 .

3. The hyaluronate nonwoven fabric according to claim 1, It is characterized in that The adhesive force of the hyaluronate nonwoven fabric is 0.9 to 2.7 kPa.

4. The hyaluronate nonwoven fabric according to claim 1, It is characterized in that The thickness of the hyaluronate nonwoven fabric is 1 to 10 mm.

5. The hyaluronate nonwoven fabric according to claim 1, It is characterized in that The tensile strength of the hyaluronate nonwoven fabric is 0.3 to 1.5 kg / mm 2 .

6. The hyaluronate nonwoven fabric according to claim 1, It is characterized in that The hyaluronate nonwoven fabric is used as a skin external application patch, a tissue repair biological material or an anti-adhesion covering material.

7. A method for producing a hyaluronate nonwoven fabric, It is characterized in that include: (a) a step of manufacturing hyaluronate fibers; (b) a step of curling the manufactured hyaluronate fiber; (c) a step of cutting the hyaluronate fiber imparted with curl; (d) forming a mesh using cut hyaluronate fibers; and (e) A step of subjecting the formed hyaluronate network to needle punching.

8. The method for producing a hyaluronate nonwoven fabric according to claim 7, It is characterized in that The steps of manufacturing hyaluronate fibers include: (a-1) a step of adjusting the water content of a hyaluronate having a weight average molecular weight of 100 to 3,000 kDa to 50 to 95% by weight to produce a hyaluronate paste; (a-2) a step of melting a hyaluronate paste having an adjusted water content at 15 to 100° C. and extruding the paste through a nozzle; and (a-3) A step of drying the extruded spinning fluid to form fibers.

9. The method for producing a hyaluronate nonwoven fabric according to claim 7, It is characterized in that The tensile strength of the manufactured hyaluronate fiber is 3 to 15 kg / mm 2 .

10. The method for producing a hyaluronate nonwoven fabric according to claim 7, It is characterized in that When forming the mesh, fibers made of a polymer material selected from the group consisting of collagen, fibronectin, gelatin, chitosan, alginic acid, polylactic acid (PLA), polyglycolic acid (PGA), polylactic-co-glycolic acid (PLGA), and polycaprolactone (PCL) are mixed.

Citation Information

Patent Citations

  • Method for preparing nonwoven fabric from bamboo fibers

    CN106012289A

  • Insulation Panel Securing Device of Liquefied Natural Gas Storage Tank

    KR102150460B1

  • Method Of Producing Hyaluronic Acid Non Woven Fabric

    KR102338355B1

  • Polymer nanofiber structural body and method of producing the same

    US20150273377A1