Attached circuit and wearable device

The circuit short circuit and corrosion problems are solved by using a polyurethane-based adhesive layer of hydroxy-terminal urethane prepolymer and curing agent, providing moderate adhesion and moisture permeability, suitable for flexible devices and wearable devices.

CN118975409APending Publication Date: 2024-11-15AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030601.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The remaining monomers in the polymerization process of acrylic adhesives and silicone adhesives cause circuit short circuits and corrosion, and the discoloration problem caused by the adhesive layer on the moisture permeable support is difficult to solve.

Method used

A polyurethane-based adhesive layer formed from the reaction product of the hydroxy-terminal urethane prepolymer and the curing agent is used to ensure that the circuit does not cause short circuits and corrosion, and provides moderate adhesion and moisture permeability.

Benefits of technology

It realizes continuous excellent bonding in the circuit pattern and adhesive layer, avoids circuit short circuit and corrosion, and is suitable for flexible devices and wearable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118975409A_ABST
    Figure CN118975409A_ABST
Patent Text Reader

Abstract

Provided is an affixed circuit having a circuit pattern and an adhesive layer, which does not cause defects such as short circuit and corrosion of the circuit, and which has excellent persistence of moderate adhesive force. The attached circuit according to the present invention has a circuit pattern and an adhesive layer, and the adhesive constituting the adhesive layer contains a reaction product of a hydroxyl-terminated urethane prepolymer and a curing agent. The hydroxyl-terminated urethane prepolymer is a reaction product of an oxyalkylene polymer A having an average number of hydroxyl groups per molecule of 2.1-3.0, an oxyalkylene polymer B having a number of hydroxyl groups per molecule of 1, and a diisocyanate compound, the content of ethylene oxide units is 5 mass% or more, and the curing agent contains a polyisocyanate compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an attached circuit having a circuit pattern and an adhesive layer, and a wearable device having the attached circuit. Background Art

[0002] In flexible electronics, technology for bonding circuits to soft and flexible substrates is being used.

[0003] For example, Patent Document 1 describes a circuit board member in which a flexible film having a circuit pattern formed thereon and an adhesive layer formed of an adhesive containing an acrylic polymer (acrylic adhesive) are laminated.

[0004] In addition, it has also been proposed to use a silicone-based adhesive in the adhesive layer (for example, refer to Patent Document 2).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2004-346106

[0008] Patent Document 2: Japanese Patent Application Publication No. 2006-281488 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] For acrylic adhesives, monomers and other adhesive components remaining during polymerization may sometimes cause short circuits and corrosion of circuits. In addition, for example, when the adhesive layer is formed on a support having moisture permeability or air permeability, discoloration occurring at the contact surface between the circuit and the support may also be a problem.

[0011] In silicone-based adhesives, there is also a problem that the same circuit defects as those mentioned above that occur in acrylic-based adhesives occur due to volatilization of low-molecular siloxane.

[0012] The present invention is made to solve the above-mentioned problems, and its purpose is to provide an attached circuit having a circuit pattern and an adhesive layer, which does not cause circuit short circuits, corrosion and other problems, and has excellent sustainability of appropriate adhesive force.

[0013] Solutions for solving problems

[0014] The present invention is based on the finding that by forming an adhesive layer for attaching a circuit with a predetermined polyurethane-based adhesive, problems such as short circuits and corrosion of the circuit do not occur and the sustainability of appropriate adhesive strength is good.

[0015] The present invention provides the following means.

[0016] [1] An attached circuit having a circuit pattern and an adhesive layer, wherein the adhesive constituting the adhesive layer comprises a reaction product of a hydroxyl-terminated urethane prepolymer and a curing agent, the hydroxyl-terminated urethane prepolymer being a reaction product of an oxyalkylene polymer A having an average number of hydroxyl groups of 2.1 to 3.0 per molecule and an oxyalkylene polymer B having a number of hydroxyl groups of 1 per molecule, and a diisocyanate compound, and the content of ethylene oxide units is 5% by mass or more, and the curing agent comprises a polyisocyanate compound.

[0017] [2] The attached circuit according to [1], wherein the number average molecular weight of the oxyalkylene polymer B is 3500 or more.

[0018] [3] The attached circuit according to [1] or [2], wherein the amount of the oxyalkylene polymer A1 having 3 hydroxyl groups per molecule is 20 parts by mass or more per 100 parts by mass of the oxyalkylene polymer A.

[0019] [4] The attached circuit according to any one of [1] to [3], wherein the content of ethylene oxide units in the oxyalkylene polymer A is 10% by mass or more.

[0020] [5] The attached circuit according to any one of [1] to [4], wherein the amount of polymer A blended is 10 to 95 parts by mass relative to 100 parts by mass of the total of polymer A and polymer B.

[0021] [6] The attached circuit according to any one of [1] to [5], wherein the polyisocyanate compound has three or more isocyanate groups in one molecule.

[0022] [7] The attached circuit according to any one of [1] to [6], wherein the thickness of the adhesive layer is 5 to 100 μm.

[0023] [8] The attached circuit according to any one of [1] to [7], wherein the moisture permeability of the adhesive layer is 3000 g / (m 2 ·day) or more.

[0024] [9] The attached circuit according to any one of [1] to [8], wherein the adhesive layer is formed on a main surface of a sheet-like support.

[0025]

[10] The attached circuit according to [9], wherein the adhesive layer is formed on one main surface of the support, and the circuit pattern is formed on the other main surface of the support.

[0026]

[11] The attached circuit according to any one of [1] to

[10] , wherein the circuit pattern is formed of conductive ink.

[0027]

[12] A wearable device comprising the attached circuit according to any one of [1] to

[11] .

[0028] Effects of the Invention

[0029] According to the present invention, it is possible to provide a bonded circuit having a circuit pattern and an adhesive layer, in which problems such as circuit short circuit and corrosion do not occur and in which a moderate adhesive force is excellent in sustainability.

[0030] The attached circuit of the present invention is suitable for flexible devices, and the adhesive layer has a low load on the skin and can exert good fixation of the circuit, etc., so it can be suitably applied to wearable devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic cross-sectional view of a bonding circuit according to the first embodiment of the present invention.

[0032] Figure 2 It is a schematic cross-sectional view of a bonding circuit according to a second embodiment of the present invention.

[0033] Figure 3 It is a schematic cross-sectional view of a bonded circuit according to a third embodiment of the present invention.

[0034] Figure 4 It is a schematic cross-sectional view of a bonding circuit according to a fourth embodiment of the present invention.

[0035] Figure 5 It is a schematic cross-sectional view of a bonded circuit according to a fifth embodiment of the present invention.

[0036] Figure 6 It is a schematic cross-sectional view of a bonding circuit according to a sixth embodiment of the present invention. DETAILED DESCRIPTION

[0037] The definitions and meanings of the terms and expressions in this specification are shown below.

[0038] The number average molecular weight (Mn) and the weight average molecular weight (Mw) are polystyrene-equivalent molecular weights determined by gel permeation chromatography (GPC) measurement based on a calibration curve prepared using a standard polystyrene sample.

[0039] The hydroxyl value-converted molecular weight is a value calculated from the calculation formula of 56100×(the number of hydroxyl groups in one molecule) / (hydroxyl value [mgKOH / g]).

[0040] The hydroxyl value is determined by measurement in accordance with JIS K1557:2007-1.

[0041] The degree of unsaturation is determined by measurement in accordance with JIS K1557-3:2007.

[0042] The isocyanate index is the equivalent ratio of isocyanate groups that react to active hydrogen-containing groups (eg, hydroxyl groups) ([isocyanate groups] / [active hydrogen-containing groups]), expressed as a percentage.

[0043] The water vapor permeability is determined by measurement in accordance with JIS Z0208:1976 (cup method). Specifically, the water vapor permeability is measured by the method described in Examples.

[0044] The attached circuit of the present invention is an attached circuit having a circuit pattern and an adhesive layer, and the adhesive constituting the adhesive layer includes a reaction product of a predetermined hydroxyl-terminated urethane prepolymer and a curing agent.

[0045] The hydroxyl-terminated urethane prepolymer is a reaction product of an oxyalkylene polymer A having an average hydroxyl number of 2.1 to 3.0 per molecule (hereinafter, also referred to as "polymer A"), an oxyalkylene polymer B having a hydroxyl number of 1 per molecule (hereinafter, also referred to as "polymer B"), and a polyisocyanate compound, and the content of ethylene oxide (EO) units is 5% by mass or more. In addition, the curing agent contains a polyisocyanate compound.

[0046] By forming the adhesive layer with the above-described predetermined polyurethane-based adhesive, it is possible to configure an attached circuit that does not cause problems such as short circuits and corrosion of the circuit and has good sustainability of appropriate adhesive strength.

[0047] [Adhesive layer]

[0048] The adhesive layer is formed of an adhesive containing a reaction product of a predetermined hydroxyl-terminated urethane prepolymer and a curing agent. A polyurethane-based adhesive formed of such a urethane prepolymer is suitable for bonding circuits in terms of circuit formation and adhesive strength.

[0049] The adhesive layer is formed by coating, attaching, etc., to a support, a circuit pattern, or a base material of a circuit pattern, etc., which are components of the adhesive sheet in an embodiment of attaching a circuit described later.

[0050] (Hydroxy-terminated urethane prepolymer)

[0051] The hydroxyl-terminated urethane prepolymer in the present invention is a reaction product of polymer A and polymer B with a diisocyanate compound. In the reaction product, the hydroxyl groups of polymer A and polymer B react with the isocyanate groups of the diisocyanate compound to form urethane bonds, and the unreacted hydroxyl groups correspond to the terminal hydroxyl groups of the hydroxyl-terminated urethane prepolymer.

[0052] The content of the EO unit in the hydroxyl-terminated urethane prepolymer is 5% by mass or more, preferably 10 to 80% by mass, and more preferably 12 to 50% by mass. By making the content of the EO unit in the hydroxyl-terminated urethane prepolymer within the above range, it is easy to obtain an adhesive layer with good adhesion that has a low load on the skin and exhibits good fixation properties for circuits, etc.

[0053] The EO units in the hydroxyl-terminated urethane prepolymer are derived from the EO units constituting polymer A and the EO units constituting polymer B. 13 The monomer composition of the oxyalkylene chain in the hydroxyl-terminated urethane prepolymer was analyzed by C-NMR (nuclear magnetic resonance) measurement to determine the content.

[0054] It should be noted that the EO unit content in the adhesive layer is also determined by the same method as the EO unit content in the hydroxyl-terminated urethane prepolymer. 13 The content is preferably 5% by mass or more, more preferably 10 to 80% by mass, and even more preferably 12 to 50% by mass, from the viewpoint of good moisture permeability, low load on the skin, and good fixation to circuits, etc., as determined by C-NMR measurement.

[0055] <Oxyalkylene polymer A>

[0056] The average number of hydroxyl groups per molecule of the oxyalkylene polymer A is 2.1 to 3.0, preferably 2.2 to 2.9, more preferably 2.3 to 2.8.

[0057] When the average hydroxyl number of the polymer A is within the above range, it is easy to obtain a pressure-sensitive adhesive layer that has good moisture permeability, is unlikely to produce adhesive residue, has a low load on the skin, and exhibits good fixation properties to circuits and the like and good adhesive strength.

[0058] The average number of hydroxyl groups per molecule of the polymer A can be calculated from the measured values ​​of the hydroxyl value and Mn of the polymer A using the calculation formula: hydroxyl value×Mn / 56100.

[0059] The polymer A may be one type of oxyalkylene polymer or two or more types of oxyalkylene polymers. When the polymer A contains two or more types of oxyalkylene polymers, it is easy to adjust the good adhesive force of the pressure-sensitive adhesive layer.

[0060] The polymer A may include, for example, an oxyalkylene polymer A1 having 3 hydroxyl groups per molecule (hereinafter, also referred to as "polymer A1") and an oxyalkylene polymer A2 having 2 hydroxyl groups per molecule (hereinafter, also referred to as "polymer A2"). In addition, as long as the average hydroxyl group per molecule of the polymer A is 2.1 to 3.0, an oxyalkylene polymer having 4 or more hydroxyl groups per molecule may be a constituent component.

[0061] It should be noted that when polymer A includes polymer A1 and polymer A2, the weighted average of the number of hydroxyl groups per molecule of polymer A1 and the number of hydroxyl groups per molecule of polymer A2 based on the composition ratio (blending amount) of polymer A1 and polymer A2 can be regarded as the average hydroxyl number of polymer A.

[0062] Of the total 100 parts by mass of the polymer A, 20 parts by mass or more of the polymer A1 is preferably present, more preferably 25 to 95 parts by mass, and even more preferably 30 to 90 parts by mass, from the viewpoint of good adhesive strength of the adhesive layer and less generation of adhesive residue.

[0063] The polymer A has an Mn of preferably 1,000 to 50,000, more preferably 5,000 to 30,000, and even more preferably 8,000 to 25,000, from the viewpoint of good flexibility and adhesive strength of the adhesive layer and less generation of adhesive residue.

[0064] When Mw / Mn of polymer A is close to 1 and the molecular weight distribution is narrowed, the hydroxyl-terminated urethane prepolymer is less likely to have high viscosity and synthesis efficiency can be improved. Therefore, it is preferably less than 1.20, more preferably less than 1.13, and further preferably less than 1.10.

[0065] In addition, for polymer A, from the viewpoint of good curability of the hydroxyl-terminated urethane prepolymer and less generation of adhesive residue in the adhesive layer, the unsaturation degree is preferably 0.020 meq / g or less, more preferably 0.018 meq / g or less, further preferably 0.015 meq / g or less, and the closer to 0 meq / g, the more preferred.

[0066] When the polymer A contains two or more oxyalkylene polymers, each oxyalkylene polymer preferably has Mn, Mw / Mn and unsaturation within the above ranges.

[0067] The synthesis method of polymer A is not particularly limited, and for example, it can be obtained by subjecting a compound having a cyclic ether structure, preferably an alkylene oxide, to ring-opening addition polymerization with an initiator having two or more active hydrogens in the presence of a catalyst. When polymer A includes polymer A1 and polymer A2, a method can also be used in which an initiator having three active hydrogens and an initiator having two active hydrogens are used in combination to perform ring-opening addition polymerization of the compound having a cyclic ether structure, thereby simultaneously generating polymer A1 and polymer A2. From the viewpoint of more correctly adjusting the blending amounts of polymer A1 and polymer A2, it is preferred to separately synthesize polymer A and polymer B and mix them, wherein polymer A is obtained by subjecting a compound having a cyclic ether structure to ring-opening addition polymerization with an initiator having three active hydrogens, and polymer B is polymer B obtained by subjecting a compound having a cyclic ether structure to ring-opening addition polymerization with an initiator having two active hydrogens.

[0068] The compound having a cyclic ether structure is preferably linear or branched and has 2 to 14 carbon atoms, more preferably 2 to 10 carbon atoms, and even more preferably 2 to 4 carbon atoms. The compound having a cyclic ether structure may be used alone or in combination of two or more.

[0069] Examples of the compound having a cyclic ether structure include ethylene oxide (EO), propylene oxide (PO), 1,2-butylene oxide, 2,3-butylene oxide, methyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, lauryl glycidyl ether, hexyl glycidyl ether, tetrahydrofuran, etc. Among these, EO and PO are preferred.

[0070] When two or more compounds having a cyclic ether structure are used in combination, in the polymer A, the arrangement of the oxyalkylene groups derived from the compounds may be random or block-like.

[0071] The polymer A preferably contains an EO unit (oxymethylene) from the viewpoint of having moderate hydrophilicity in consideration of good adhesion to the skin and obtaining an adhesive layer with suppressed crystallinity, and more preferably contains 10% by mass or more, further preferably contains 15 to 60% by mass, and further preferably contains 20 to 50% by mass.

[0072] The content of EO units in polymer A can be determined by 13 C-NMR measurement is performed to analyze and determine the monomer composition of the oxyalkylene chain in the polymer A. For example, when the oxyalkylene chain in the polymer A includes EO units and PO units, the EO unit content can be calculated based on the area of ​​the peak representing the methylene group of the EO unit and the area of ​​the peak representing the methyl group of the PO unit.

[0073] When the polymer A includes the polymer A1 and the polymer A2, the same applies to the EO unit content of each of the polymer A1 and the polymer A2.

[0074] It should be noted that the content of EO units in polymer A can be regarded as a value calculated from the amount of ethylene oxide in the synthetic raw material of polymer A. In the case where polymer A includes polymer A1 and polymer A2, the value obtained by weighted average of the EO unit content of polymer A1 and the EO unit content of polymer A2 based on the composition ratio (blend amount) of polymer A1 and polymer A2 can be regarded as the EO unit content of polymer A.

[0075] Examples of the group having active hydrogen in the initiator include a hydroxyl group, a carboxyl group, an amino group having a hydrogen atom bonded to a nitrogen atom, etc. Among these, a hydroxyl group is preferred, and an alcoholic hydroxyl group is more preferred.

[0076] Examples of the initiator having three hydroxyl groups include glycerin, trimethylolethane, trimethylolpropane, 1,2,6-hexanetriol, etc. Among these, one type may be used alone, or two or more types may be used in combination.

[0077] Examples of the initiator having two hydroxyl groups include ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol. Among these, one type may be used alone, or two or more types may be used in combination.

[0078] The number of active hydrogen atoms in the initiator is generally equivalent to the number of hydroxyl groups per molecule of the oxyalkylene polymer. The polymer A1 can be synthesized using, for example, glycerol as an initiator. The polymer A2 can be synthesized using, for example, propylene glycol as an initiator.

[0079] It should be noted that the initiator of the synthetic raw material of the oxyalkylene polymer can be 13 When polymer A includes polymer A1 and polymer A2, the type and amount of polymer A are determined by 13 The information on the types and amounts of the initiators obtained by C-NMR measurement was used to determine the content ratios of oxyalkylene groups such as EO units and PO units bonded to the respective initiators, and the ratio of polymer A1 to polymer A2 was determined.

[0080] Ring-opening addition polymerization can be carried out using known catalysts such as alkali catalysts such as potassium hydroxide, transition metal compound-porphyrin complex catalysts such as complexes obtained by reacting organoaluminum compounds with porphyrin, composite metal cyanide complex catalysts, catalysts comprising phosphazene compounds, etc. Among these catalysts, composite metal cyanide complex (DMC) catalysts are preferred from the aspect of obtaining oxyalkylene polymers with narrow molecular weight distribution and low viscosity. As composite metal cyanide complexes, known compounds can be used, for example, zinc hexacyanocobaltate complexes with tert-butyl alcohol as ligands can be cited.

[0081] The synthesis of the oxyalkylene polymer by ring-opening addition polymerization using a DMC catalyst can be carried out by a known method, for example, the production methods described in International Publication No. 2003 / 062301, International Publication No. 2004 / 067633, Japanese Patent Application Publication No. 2004-269776, Japanese Patent Application Publication No. 2005-15786, International Publication No. 2013 / 065802, Japanese Patent Application Publication No. 2015-10162, etc. can be applied.

[0082] <Oxyalkylene polymer B>

[0083] The number of hydroxyl groups per molecule of the oxyalkylene polymer B is 1. The polymer B may be one type of oxyalkylene polymer or two or more types of oxyalkylene polymers.

[0084] The number of hydroxyl groups in polymer B can be determined in the same manner as in polymer A by using 13 The type and amount of the initiator in the synthetic raw materials were confirmed by C-NMR measurement.

[0085] The polymer B preferably has an Mn of 3,500 or more, more preferably 4,000 to 50,000, and even more preferably 4,500 to 30,000, from the viewpoint of good flexibility of the pressure-sensitive adhesive layer and good followability when attached to the skin.

[0086] When Mw / Mn of polymer B is close to 1 and the molecular weight distribution is narrow, the hydroxyl-terminated urethane prepolymer is less likely to have high viscosity and synthesis efficiency can be improved. Therefore, it is preferably less than 1.20, more preferably less than 1.13, and further preferably less than 1.10.

[0087] In addition, for polymer B, from the viewpoint of good curability of the hydroxyl-terminated urethane prepolymer and less generation of residual adhesive in the adhesive layer, the unsaturation degree is preferably 0.015 meq / g or less, more preferably 0.013 meq / g or less, and further preferably 0.010 meq / g or less, and the closer to 0 meq / g, the more preferred.

[0088] When the polymer B contains two or more oxyalkylene polymers, each oxyalkylene polymer preferably has Mn, Mw / Mn and unsaturation within the above ranges.

[0089] The polymer B is not particularly limited in its synthesis method, and can be obtained, for example, by subjecting a compound having a cyclic ether structure, preferably an alkylene oxide, to ring-opening addition polymerization with an initiator having one active hydrogen in the presence of a catalyst.

[0090] The compound having a cyclic ether structure is the same as described for the polymer A. It is preferred to use PO alone or a combination of EO and PO.

[0091] The polymer B preferably has an EO unit content of 0 to 80% by mass, more preferably 0 to 60% by mass, and even more preferably 0 to 50% by mass, from the viewpoint of having an appropriate moisture permeability in consideration of good adhesion to the skin and obtaining a pressure-sensitive adhesive layer with suppressed crystallinity.

[0092] The content of the EO unit in the polymer B was determined in the same manner as in the case of the polymer A.

[0093] Examples of the group having active hydrogen in the initiator include the same groups as those in the case of the polymer A, and a hydroxyl group is preferred, and an alcoholic hydroxyl group is more preferred.

[0094] As the initiator having one hydroxyl group, monohydric alcohols having 2 to 4 carbon atoms are preferred from the viewpoint of availability, etc., and examples thereof include n-propanol, isopropanol, n-butanol, sec-butanol, isobutanol, tert-butanol, etc. Among these, n-butanol, sec-butanol, isobutanol, and tert-butanol are preferred. The initiator may be used alone or in combination of two or more.

[0095] The ring-opening addition polymerization can be carried out in the same manner as in the case of the polymer A by a known method.

[0096] <Diisocyanate Compound>

[0097] The diisocyanate compound used in the synthesis of the hydroxyl-terminated urethane prepolymer is an organic compound having two isocyanate groups in one molecule. The diisocyanate compound may be used alone or in combination of two or more.

[0098] As the diisocyanate compound, as an aliphatic diisocyanate compound, any of linear or branched ones can be mentioned, for example, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, 3-methylpentane-1,5-diisocyanate, etc.

[0099] Examples of the alicyclic diisocyanate compound include isophorone diisocyanate (IPDI), hydrogenated xylylene diisocyanate, 4,4′-dicyclohexylmethane diisocyanate (HMDI), 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, and 1,3-bis(isocyanatemethyl)cyclohexane.

[0100] Examples of the aromatic diisocyanate compound include toluene diisocyanate, 2,2′-diphenylmethane diisocyanate, 2,4′-diphenylmethane diisocyanate, 4,4′-diphenylmethane diisocyanate (MDI), 4,4′-dibenzyl diisocyanate, 1,5-naphthalene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, dialkyl diphenylmethane diisocyanate, and tetraalkyl diphenylmethane diisocyanate.

[0101] Moreover, as an aromatic aliphatic diisocyanate compound, xylylene diisocyanate, tetramethylxylylene diisocyanate (TMXDI), etc. are mentioned, for example.

[0102] Among these, HDI, IPDI, HMDI, and TMXDI are preferred, and HDI is more preferred, from the viewpoint of obtaining a pressure-sensitive adhesive layer having a high glass transition temperature and good tensile strength and elongation at break.

[0103] Alternatively, as the diisocyanate compound, a bifunctional isocyanate-terminated urethane prepolymer obtained by reacting the above-mentioned diisocyanate compound with a diol (e.g., ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, etc.) in advance may be used.

[0104] <Synthesis method>

[0105] The hydroxyl-terminated urethane prepolymer can be synthesized, for example, by a method in which polymer A, polymer B, a diisocyanate compound, and a catalyst and a solvent appropriately added as needed are all put into a reaction vessel at once; and a method in which a diisocyanate compound is added dropwise to a reaction vessel in which polymer A and polymer B, and a catalyst and a solvent appropriately added as needed are put. From the viewpoint of the ease of controlling the molecular weight distribution of the hydroxyl-terminated urethane prepolymer based on the preferential reaction of low molecular weight components in the synthetic raw materials, the method of adding a diisocyanate compound is preferred.

[0106] As the catalyst, a known urethanization catalyst such as a tertiary amine compound, an organic metal compound, etc. can be used. The catalyst may be used alone or in combination of two or more.

[0107] Examples of the tertiary amine compound include triethylamine, triethylenediamine, and 1,8-diazabicyclo[5.4.0]-7-undecene (DBU).

[0108] Examples of the organometallic compound include tin compounds such as dibutyltin dichloride, dibutyltin oxide, dibutyltin dibromide, dibutyltin dimaleate, dibutyltin dilaurate (DBTDL), dibutyltin diacetate, dibutyltin sulfide, tributyltin sulfide, tributyltin oxide, tributyltin acetate, triethyltin ethoxide, tributyltin ethoxide, dioctyltin oxide, tributyltin chloride, tributyltin trichloroacetate, and tin 2-ethylhexanoate; titanium compounds such as dibutyltitanium dichloride, tetrabutyl titanate, and butoxytitanium trichloride; lead compounds such as lead oleate, lead 2-ethylhexanoate, lead benzoate, and lead naphthenate; iron compounds such as iron 2-ethylhexanoate and iron acetylacetonate; cobalt compounds such as cobalt benzoate and cobalt 2-ethylhexanoate; zinc compounds such as zinc naphthenate and zinc 2-ethylhexanoate; zirconium compounds such as zirconium naphthenate, and the like.

[0109] When a catalyst is used, the amount used is preferably 0.001 to 1.0 part by mass, more preferably 0.002 to 0.5 part by mass, and even more preferably 0.005 to 0.1 part by mass based on 100 parts by mass of the total of the polymer A and the polymer B, from the viewpoint of appropriately promoting the urethanization reaction.

[0110] Examples of the solvent include ketones such as acetone and methyl ethyl ketone; esters such as ethyl acetate; and aromatic hydrocarbons such as toluene and xylene. The solvent may be used alone or in combination of two or more.

[0111] When a solvent is used, the amount thereof is preferably 50 to 500 parts by mass, more preferably 70 to 400 parts by mass, and even more preferably 80 to 300 parts by mass based on 100 parts by mass of the total of polymer A and polymer B from the viewpoint of uniformity of the reaction system and synthesis efficiency.

[0112] From the viewpoint of obtaining an adhesive layer having moderate moisture permeability while taking into account good adhesion to the skin, the blending amount of polymer A is preferably 10 to 95 parts by mass, more preferably 20 to 90 parts by mass, and further preferably 30 to 85 parts by mass, relative to 100 parts by mass of the total of polymer A and polymer B.

[0113] From the viewpoint of efficiently obtaining a hydroxy-terminated urethane prepolymer having an appropriate molecular chain length, it is preferred that the polymer A, the polymer B and the diisocyanate compound be reacted at an isocyanate index of less than 100, preferably 30-95, more preferably 50-95.

[0114] The reaction temperature is preferably lower than 100°C, more preferably 70 to 95°C, and even more preferably 75 to 90°C, from the viewpoint of promoting the urethanization reaction and suppressing the side reaction.

[0115] After the reaction is completed, a reaction terminator such as acetylacetone may be added to deactivate the catalyst.

[0116] The average number of hydroxyl groups per molecule of the hydroxyl-terminated urethane prepolymer is preferably less than 3.0, more preferably 1.7 to 2.9, and even more preferably 1.8 to 2.5, from the viewpoint of obtaining a pressure-sensitive adhesive layer having an appropriate moisture permeability while allowing for good adhesion to the skin.

[0117] The average number of hydroxyl groups per molecule of the hydroxyl-terminated urethane prepolymer can be regarded as a weighted average of the average number of hydroxyl groups per molecule of polymer A and the average number of hydroxyl groups per molecule of polymer B based on the composition ratio (compounding amount) of polymer A and polymer B.

[0118] (Curing agent)

[0119] The adhesive constituting the adhesive layer is obtained by reacting the hydroxyl-terminated urethane prepolymer with a curing agent. The curing agent includes a polyisocyanate compound having two or more isocyanate groups in one molecule. The polyisocyanate compound may be used alone or in combination of two or more.

[0120] As the polyisocyanate compound, diisocyanate compounds are preferred from the viewpoints of availability, reactivity, etc. In addition, polyisocyanate compounds having three or more isocyanate groups in one molecule are preferred from the viewpoints of good adhesion of the adhesive layer and difficulty in producing residual adhesive.

[0121] Specific examples of the diisocyanate compound include the same specific examples as those of the diisocyanate compound constituting the above-mentioned hydroxyl-terminated urethane prepolymer.

[0122] Examples of the polyisocyanate compound include derivatives of the above-mentioned diisocyanate compounds, such as isocyanurate-modified products (e.g., "CORONATE (registered trademark; hereinafter omitted) HX" (manufactured by Tosoh Corporation)), biuret-modified products (e.g., "DURANATE (registered trademark) 24A-100" (manufactured by Asahi Kasei Corporation)), allophanate-modified products, and reaction products of diisocyanate compounds with a polyol having three or more hydroxyl groups in one molecule (e.g., trimethylolpropane), i.e., trifunctional or higher isocyanate-terminated urethane prepolymers (adducts) (e.g., "CORONATE L", "CORONATE L-55E", "CORONATE L-45E" (all manufactured by Tosoh Corporation)).

[0123] The isocyanate index of the polyisocyanate compound to be reacted with the hydroxyl-terminated urethane prepolymer is preferably more than 100, more preferably 101 to 1500, and even more preferably 105 to 1000.

[0124] (Adhesive)

[0125] The adhesive used for forming the adhesive layer may be a one-component type in which a hydroxyl-terminated urethane prepolymer and a curing agent are mixed in advance, or may be a two-component type including a first component containing a hydroxyl-terminated urethane prepolymer and a second component containing a curing agent.

[0126] In the synthesis of the reaction product of the hydroxy-terminated urethane prepolymer and the curing agent, a catalyst and a solvent may be used as necessary.

[0127] As the catalyst, the above-mentioned urethanization catalyst can be used. In addition, when a catalyst is used, its amount is preferably 0.001 to 1.0 parts by mass, more preferably 0.002 to 0.5 parts by mass, and further preferably 0.005 to 0.1 parts by mass relative to 100 parts by mass of the total of the hydroxyl-terminated urethane prepolymer and the curing agent. It is preferred that a reaction terminator is added after the reaction is completed to deactivate the catalyst.

[0128] As the solvent, the same solvent as that used in the synthesis of the hydroxyl-terminated urethane prepolymer can be used. When a solvent is used, the amount thereof is preferably 50 to 500 parts by mass, more preferably 70 to 400 parts by mass, and even more preferably 80 to 300 parts by mass, relative to 100 parts by mass of the total of the hydroxyl-terminated urethane prepolymer and the curing agent.

[0129] From the viewpoint of promoting the urethanization reaction and suppressing the side reaction, the reaction temperature is preferably lower than 120°C, more preferably 40 to 110°C, and even more preferably 50 to 100°C.

[0130] (Other ingredients)

[0131] The adhesive may include other components other than the reaction product of the hydroxyl-terminated urethane prepolymer and the curing agent. As other components, for example, various additives such as plasticizers, antioxidants, antistatic agents, fillers, ultraviolet absorbers, light stabilizers, conductivity imparting agents, and leveling agents may be cited. In addition, solvents may also be included. These other components in the adhesive may be a single one, or two or more may be used in combination, and may be mixed in a content within a range that does not damage the effect of the present invention.

[0132] The plasticizer can be selected from the viewpoints of compatibility with other components, wettability of the pressure-sensitive adhesive layer to an adherend, and the like, and examples thereof include fatty acid esters and phosphoric acid esters having 8 to 30 carbon atoms.

[0133] The antioxidant contributes to the suppression of thermal degradation of the pressure-sensitive adhesive layer, and examples thereof include phenolic, amine, sulfur, and phosphorus antioxidants. Among these, phenolic antioxidants are preferred because of their low skin sensitization potential.

[0134] The antistatic agent contributes to the suppression of damage to the circuit pattern due to electrostatic discharge, and examples thereof include inorganic salts; ionic liquids containing imidazolium ions, pyridinium ions, ammonium ions, and the like; and surfactants.

[0135] Examples of the filler include talc, calcium carbonate, and titanium oxide.

[0136] Examples of the ultraviolet absorber include benzophenone-based, benzotriazole-based, salicylic acid-based, oxalic anilide-based, cyanoacrylate-based, and triazine-based ultraviolet absorbers.

[0137] Examples of the light stabilizer include hindered amine light stabilizers and ultraviolet light stabilizers.

[0138] Examples of the conductivity-imparting agent include metal fine particles such as silver nanoparticles.

[0139] (Moisture Permeability)

[0140] The moisture permeability of the adhesive layer is preferably 3000 g / (m 2 ·day) or more, more preferably 3500g / (m 2 ·day) or more, more preferably 4000 (g / m 2 The upper limit of the moisture permeability is not particularly limited.

[0141] It should be noted that the moisture permeability in the present invention is a measured value at 40°C and 90% RH atmosphere, and is a value at a thickness of 25 μm for the adhesive layer. Specifically, the measurement is performed by the method described in the Examples. In the Examples, the moisture permeability of the adhesive sheet including the support of the adhesive layer is also compared with the moisture permeability of commercially available adhesive sheets.

[0142] (Adhesion)

[0143] When the adhesive force of the adhesive layer to human skin is preferably 0.2 to 1.0 N / 15 mm, more preferably 0.3 to 0.7 N / 15 mm, it can be said that the adhesive layer has a low load on the skin and has good adhesive force.

[0144] In addition, when the adhesive layer is bonded to a sealing material of a circuit pattern, for example, if the adhesive force to the common material of the sealing material, i.e., phenolic resin, is greater than the adhesive force to human skin, and is preferably 2.0 N / 15 mm or more, and more preferably 3.0 N / 15 mm or more, then it can be said that the adhesive layer can exert good fixation of the circuit, etc.

[0145] In addition, the adhesive force mentioned here is a value measured by the method based on JIS Z0237:2009, and is specifically measured by the method described in the Example.

[0146] (Storage modulus)

[0147] The storage modulus of the adhesive layer at 25°C is preferably 1.0×10 4 ~5.0×10 5 Pa, more preferably 2.0×10 4 ~4.0×10 5 Pa, more preferably 3.0×10 4 ~3.0×10 5 Pa.

[0148] From the same viewpoint, the storage modulus at 80°C is preferably 4.0×10 5 Pa or less, more preferably 5.0×10 2 ~3.0×10 5 Pa, more preferably 1.0×10 3 ~6.0×10 4 Pa.

[0149] The storage modulus mentioned here is a value measured using a dynamic viscoelasticity measuring device (measurement conditions: tensile mode, strain 1%, temperature range -80 to 130°C, heating rate 3°C / min, frequency 1 Hz, sample: diameter 3 mm×length 4 cm).

[0150] [Circuit pattern]

[0151] The circuit pattern is formed of a conductive material, and as a method for forming a circuit pattern on a substrate, etc., it can be formed by a known method. For example, it can be formed by a subtractive method in which a metal film is processed into a pattern shape by etching, a full-additive method using resist formation and plating technology, a semi-additive method, a method of printing into a pattern shape using conductive ink (for example, silver paste, etc.), etc. Among these, from the viewpoints of the retainability of the circuit in the application of the adhesive of the present invention, the ease of forming a fine circuit, etc., it is preferred to form a circuit pattern by a method using conductive ink.

[0152] The substrate used for forming the circuit pattern can be a known material, for example, paper or glass cloth impregnated with a phenolic resin or an epoxy resin. In the production of a flexible attached circuit, for example, a film of polyimide or polyester is suitably used.

[0153] [Structure of attached circuit]

[0154] As an embodiment of the attached circuit of the present invention, for example, there can be mentioned Figures 1 to 6 The structure is as shown in the cross-sectional schematic diagram of the present invention, but it is not limited to these examples. Hereinafter, as a preferred embodiment that can exert the effect of the present invention, the method of using skin as an adherend is described, but the adherend of the attached circuit of the present invention is not limited to skin, and all solids can be used as objects.

[0155] (First embodiment)

[0156] exist Figure 1 In the attached circuit of the first embodiment shown, an adhesive sheet having an adhesive layer 11 formed on the main surface of a sheet-like support 12 is used. The attached circuit can be attached to the skin 40 by covering a packaged device 22 having a circuit pattern 21 and an insulating layer 23 formed on a substrate in advance and sealed with the adhesive sheet so that the packaged device 22 and the adhesive layer 11 around it are in contact with the skin 40 and the adhesive layer 11 is pressed against the skin 40.

[0157] The support 12 used in the adhesive sheet is preferably formed of a material that has good conformability to the shape of the packaged device 22 or the skin 40 and can obtain sufficient breaking strength even in a thin layer, and examples thereof include supports formed of resin films, cloth, paper, etc. The material of the support 12 may be a single type or a combination of two or more types, and may also be a composite material based on lamination or the like.

[0158] Examples of the material of the resin film include polyurethane, polyamide, acrylic resin, polyolefins such as polyethylene, polypropylene, and ethylene-vinyl acetate copolymer, and polyester. Among these, polyurethane and polyamide are preferred from the viewpoint of good moisture permeability.

[0159] Examples of the cloth include woven cloth, nonwoven cloth, knitted cloth, and net, and the material may be the resin of the material of the resin film, or natural fibers such as cotton, silk, and wool.

[0160] The thickness of the support 12 is not particularly limited as long as it can ensure conformability to the shape of the package device 22 or the skin 40 and has sufficient breaking strength, and is, for example, 10 to 500 μm.

[0161] The thickness of the pressure-sensitive adhesive layer 11 in the pressure-sensitive adhesive sheet is preferably 5 to 100 μm, more preferably 10 to 80 μm, and even more preferably 20 to 50 μm from the viewpoint of ensuring good adhesion to the skin and moisture permeability.

[0162] The surface of the adhesive layer 11 of the adhesive sheet is preferably covered with a release liner for protecting the surface of the adhesive layer 11 before being attached to the skin 40 .

[0163] The release liner may be one used in known skin adhesive tapes, etc. For example, there may be high-quality paper, glassine paper, parchment paper coated with a release agent such as silicone resin or fluororesin on the surface, and high-quality paper coated with a resin anchor coating or polyethylene lamination and coated with a release agent such as silicone resin or fluororesin on the surface.

[0164] The release liner is appropriately released from the surface of the pressure-sensitive adhesive layer 11 to use the pressure-sensitive adhesive sheet.

[0165] (Second embodiment)

[0166] exist Figure 2In the attached circuit of the second embodiment shown, the same adhesive sheet as in the first embodiment is used, an adhesive layer 11 is formed on one main surface of a support 12, and a circuit pattern 21 is formed on the other main surface of the support 12 on the opposite side of the adhesive layer 11. In this embodiment, the support 12 also serves as a base material for the circuit pattern 21, which is advantageous in terms of thin filmization, flexibility, and conformability to the shape of the skin 40 of the attached circuit.

[0167] In order to directly form the circuit pattern 21 on the surface of the support 12 , among the above-mentioned circuit pattern forming methods, it is more preferable to use a method such as printing using conductive ink (for example, silver paste, etc.).

[0168] exist Figure 2 In the embodiment, the circuit pattern 21 on the support 12 is covered with the insulating layer 23, but the insulating layer 23 may not be formed depending on the purpose of use of the attached circuit. The method for forming the insulating layer 23 is not particularly limited, and for example, coating with a solder resist may be used.

[0169] (Third embodiment)

[0170] exist Figure 3 In the attached circuit of the third embodiment shown, a circuit pattern 21 is formed on the surface of the adhesive layer 11. In this embodiment, the support 12 is not used, so compared with the first and second embodiments, the attached circuit is more advantageous in terms of thin film, flexibility, and conformability to the shape of the skin 40.

[0171] In addition, when the adhesive layer 11 has conductivity, the patch circuit of this embodiment can also be used in a state where the circuit pattern 21 and the skin 40 are in a conductive state.

[0172] In order to directly form the circuit pattern 21 on the surface of the adhesive layer 11 , among the above-mentioned circuit pattern forming methods, it is more preferable to use a method such as printing using conductive ink (for example, silver paste, etc.).

[0173] Since the adhesive layer 11 in this embodiment is not formed on the support 12, it is preferable that both sides of the adhesive layer 11 are covered with the above-mentioned release liner in order to protect both sides before the formation of the circuit pattern 21 and the attachment to the skin 40. The adhesive layer 11 formed in this way without using the support 12 is called an adhesive transfer sheet. The release liner is appropriately peeled off from the surface of the adhesive layer 11 to use the adhesive transfer sheet.

[0174] exist Figure 3 In the embodiment, the circuit pattern 21 on the adhesive layer 11 is covered with the insulating layer 23, but the insulating layer 23 may not be formed depending on the purpose of use of the attached circuit. The method for forming the insulating layer 23 is the same as that of the second embodiment.

[0175] (Fourth embodiment)

[0176] exist Figure 4 In the attached circuit of the fourth embodiment shown, the main surface of the substrate 22 on which the circuit pattern 21 is formed is bonded to the surface of the adhesive layer 11. Unlike the first embodiment, the adhesive transfer sheet is used so that the circuit substrate on which the circuit pattern 21 is formed on the substrate 22 is not in direct contact with the skin 40, and the adhesive layer 11 is pressed against the skin 40, thereby making it possible to attach the attached circuit to the skin 40.

[0177] exist Figure 4 In the embodiment, the circuit pattern 21 on the substrate 22 is covered with the insulating layer 23, but the insulating layer 23 may not be formed depending on the purpose of use of the attached circuit. The method of forming the insulating layer 23 is the same as that of the second embodiment.

[0178] (Fifth embodiment)

[0179] exist Figure 5 In the attached circuit of the fifth embodiment shown, the circuit pattern 21 formed on the base material 22 is bonded to the surface of the adhesive layer 11 with the surface opposite to the base material 22 .

[0180] When the pressure-sensitive adhesive layer 11 has conductivity, the patch circuit of this embodiment can also be used in a manner that the circuit pattern 21 and the skin 40 are in a conductive state, similarly to the second embodiment.

[0181] exist Figure 5 In the embodiment, the circuit pattern 21 (shown on the lower side in the figure) on the substrate 22 is covered with an insulating layer 23, but the insulating layer 23 may not be formed depending on the purpose of use of the attached circuit. The method for forming the insulating layer 23 is the same as that of the second embodiment.

[0182] In addition, the insulating layer 23 is not limited to covering the entire circuit pattern 21, and may also be Figure 5 When the adhesive layer 11 has conductivity, the patch circuit of this form can be applied in a state where a part of the circuit pattern 21 is electrically connected to the skin 40 via the adhesive layer 11.

[0183] (Sixth embodiment)

[0184] exist Figure 6In the attached circuit of the sixth embodiment shown, the adhesive layer 11 is formed on one main surface of the support 12 using the same adhesive sheet as the first embodiment, and the package device 22, which is the same as the first embodiment, is adhered to the other main surface of the support 12 on the opposite side of the adhesive layer 11 by another adhesive layer 31. Unlike the first embodiment, the attached circuit of this embodiment can be attached to the skin 40 in a state where only the adhesive layer 11 contacts the skin 40 without the circuit pattern 21 sealed as the package device 22 contacting the skin 40.

[0185] The other adhesive layer 31 is not particularly limited as long as it has an adhesive force sufficient to fix the package device 22 to the main surface of the support body 12 , and a known adhesive, double-sided tape, etc. may be applied. In addition, it may be the same as the adhesive layer 11 .

[0186] [Wearable devices]

[0187] When using the above-mentioned attached circuit of the present invention, the adhesive layer has a low load on the skin, and no abnormality will occur on the skin for a long time of more than several days. It can be continuously attached, and a wearable device with good fixation of the circuit, etc. can be appropriately provided.

[0188] Examples of wearable devices attached to the skin include biosensors and environmental sensors, and examples of detection items of the biosensors include cardiac potential, pulse wave, body temperature, acceleration, heartbeat interval, pulse interval, breathing interval, electrocardiogram, electromyogram, activity level, blood pressure, body temperature, brain waves, and the like.

[0189] Example

[0190] Hereinafter, the present invention will be specifically described based on examples, but the present invention is not limited to the following examples, and various modifications can be made within the scope not departing from the gist of the present invention.

[0191] [Measurement method]

[0192] The methods for measuring various physical properties in the following Synthesis Examples and Production Examples are as follows.

[0193] (Hydroxy value)

[0194] The hydroxyl value V is determined according to method B (potentiometric automatic titration method) of JIS K1557-1:2007.

[0195] (Hydroxy value converted molecular weight)

[0196] Hydroxyl value converted molecular weight M OHV The hydroxyl value OHV [mgKOH / g] obtained above was used to calculate the hydroxyl value using the following formula.

[0197] M OHV=56.1×1000×x / OHV

[0198] In the formula, 56.1 represents the molecular weight of potassium hydroxide. x represents the number of hydroxyl groups per molecule of the oxyalkylene polymer, and the number of hydroxyl groups per molecule of the initiator used for the synthesis of the oxyalkylene polymer is regarded as x.

[0199] (Number average molecular weight (Mn) and weight average molecular weight (Mw))

[0200] Mn and Mw were measured by gel permeation chromatography (GPC) under the following measurement conditions (polystyrene conversion), and the molecular weight distribution (Mw / Mn) was calculated from these values.

[0201] [Measurement conditions]

[0202] · Machine used: "HLC-8320GPC", manufactured by Tosoh Corporation

[0203] Column used: "TSKgel (registered trademark) SuperMultiporeHZ-M", manufactured by Tosoh Corporation

[0204] Detector: Differential refractive index (RI) detector

[0205] Detection temperature: 40℃

[0206] ·Eluent: Tetrahydrofuran

[0207] Flow rate: 0.350mL / min

[0208] Sample concentration: 0.5 mass%

[0209] Sample injection volume: 10μL

[0210] Standard sample: polystyrene

[0211] (Ethylene oxide (EO) unit content)

[0212] Regarding the EO unit content of the oxyalkylene polymer, the charge amount of EO was regarded as the EO unit content in the oxyalkylene polymer based on the charge amounts of PO and EO used in the synthesis.

[0213] The EO unit content of the hydroxyl-terminated urethane prepolymer is the weighted average value of the EO unit content in each component of the raw material.

[0214] (Unsaturation)

[0215] The degree of unsaturation is measured in accordance with JIS K1557-3:2007.

[0216] (Average number of hydroxyl groups per molecule of oxyalkylene polymer A)

[0217] The value obtained by weightedly averaging the number of hydroxyl groups per molecule of each of the oxyalkylene polymers A1 and A2 used as the oxyalkylene polymer A (the number of hydroxyl groups per molecule of the initiator used for synthesis) based on the respective blending amounts of the oxyalkylene polymers A1 and A2 was defined as the average number of hydroxyl groups per molecule.

[0218] (Average number of hydroxyl groups per molecule of hydroxyl-terminated urethane prepolymer)

[0219] The value obtained by weighted average of the number of hydroxyl groups per molecule of each oxyalkylene polymer (oxyalkylene polymers A1, A2, and B) used for synthesis of the hydroxyl-terminated urethane prepolymer based on the blending amount of each oxyalkylene polymer was regarded as the average number of hydroxyl groups per molecule.

[0220] [Substances used]

[0221] Details of various substances used in the following synthesis examples are shown below.

[0222] ·TBA-DMC catalyst: zinc hexacyanocobaltate complex with tert-butyl alcohol as ligand

[0223] PO: Propylene oxide

[0224] EO: Ethylene oxide

[0225] Adsorbent: Synthetic magnesium silicate; "KYOWAAD (registered trademark) 600S", manufactured by Kyowa Chemical Industry Co., Ltd.

[0226] ·DBTDL: Dibutyltin dilaurate; manufactured by Tokyo Chemical Industry Co., Ltd.; urethanization catalyst

[0227] HDI: Hexamethylene diisocyanate; "DURANATE (registered trademark) 50M-HDI", manufactured by Asahi Kasei Corporation

[0228] Curing agent: trimethylolpropane-modified toluene diisocyanate (TDI-TMP adduct); "CORONATEL", manufactured by Tosoh Corporation; solid content: about 75% by mass

[0229] Silver paste: "TR70901", manufactured by Taiyo Ink Manufacturing Co., Ltd.

[0230] [Synthesis of oxyalkylene polymer]

[0231] (Synthesis Example 1-1)

[0232] In a pressure vessel, 1000 g of glycerol as an initiator and a TBA-DMC catalyst (metal concentration: 46 mass ppm) were placed, and after nitrogen substitution in the vessel, the reaction solution was heated to 135° C. while stirring, and 120 g of PO was added to carry out a reaction.

[0233] After the temperature rise of the reaction liquid stopped, it was cooled to 135° C., and 3782.4 g of PO and 945.6 g of EO were added to the container while stirring the reaction liquid. After confirming that the internal pressure did not change, an adsorbent was added to perform neutralization and catalyst removal to obtain an oxyalkylene polymer A1.

[0234] (Synthesis Example 1-2)

[0235] In Synthesis Example 1-1, except that the initiator was changed from glycerol to propylene glycol, the same operation as Synthesis Example 1-1 was carried out to synthesize an oxyalkylene polymer A2.

[0236] (Synthesis Example 1-3)

[0237] In Synthesis Example 1-1, an oxyalkylene polymer B1 was synthesized in the same manner as Synthesis Example 1-1 except that the initiator was changed from glycerol to n-butanol and 2364 g of PO was added instead of EO after the reaction solution was cooled.

[0238] The aspects of each oxyalkylene polymer produced in the above-mentioned synthesis example are shown in Table 1 below.

[0239] [Table 1]

[0240] Table 1

[0241] Synthesis example 1-1 1-2 1-3 Oxyalkylene polymers A1 A2 B1 Number of hydroxyl groups per molecule 3 2 1 Hydroxyl value [mgKOH / g] 17.6 11,8 11.5 Mn 8470 9510 4900 Mw / Mn 1.19 1.06 1.09 EO unit content [mass %] 20 20 0 Unsaturation [meq / g] 0.013 0.011 0.007

[0242] [Synthesis of Hydroxyl-Terminated Urethane Prepolymer]

[0243] (Synthesis example 2-1)

[0244] In a reaction container equipped with a thermometer, a stirrer and a cooling tube, 36 parts by mass of the oxyalkylene polymer A1, 48 parts by mass of the oxyalkylene polymer A2, 16 parts by mass of the oxyalkylene polymer B1, 50.6 parts by mass of toluene and 50.6 parts by mass of ethyl acetate were charged, 0.006 parts by mass of DBTDL was added, and after mixing at 40°C, 1.69 parts by mass of HDI (isocyanate index 85) was added, and the reaction was carried out at 80°C.

[0245] The average number of hydroxyl groups per molecule of the blended oxyalkylene polymer A (oxyalkylene polymers A1 and A2) was 2.4.

[0246] The mixture was appropriately diluted with ethyl acetate and kept at 80° C. to react for 7 hours to obtain a 50% by mass transparent hydroxyl-terminated urethane prepolymer (prepolymer U1; average hydroxyl number 2.1, EO unit content 17% by mass) solution.

[0247] (Synthesis example 2-2)

[0248] In a reaction container equipped with a thermometer, a stirrer and a cooling tube, 30 parts by mass of the oxyalkylene polymer A1, 70 parts by mass of the oxyalkylene polymer A2, 50.6 parts by mass of toluene and 50.6 parts by mass of ethyl acetate were charged, 0.006 parts by mass of DBTDL was added, and after mixing at 40°C, 1.69 parts by mass of HDI (isocyanate index 85) was added, and the reaction was carried out at 80°C.

[0249] The average number of hydroxyl groups per molecule of the blended oxyalkylene polymer A (oxyalkylene polymers A1 and A2) was 2.4.

[0250] The reaction was carried out for 7 hours while being appropriately diluted with ethyl acetate and kept at 80°C to obtain a 50% by mass transparent hydroxyl-terminated urethane prepolymer (prepolymer U2; average hydroxyl number 2.5, EO unit content 20% by mass) solution.

[0251] [Manufacture of PSA Sheet for Evaluation]

[0252] (Production Example 1)

[0253] 100 parts by mass of prepolymer U1 solution (concentration 50% by mass) and 10 parts by mass of curing agent (isocyanate index 500) were mixed and degassed, then coated with a knife coater (dry film thickness 25 μm) on a polyester film (thickness 50 μm) as a release liner, and dried at 100° C. for 3 minutes to form an adhesive layer. A polyester nonwoven fabric (thickness 70 μm) as a support was bonded to the adhesive layer, and cured in a hot air dryer at 50° C. for 3 days to prepare an adhesive sheet S1.

[0254] (Production Example 2)

[0255] In Production Example 1, a pressure-sensitive adhesive sheet S6 was prepared by performing the same operation as in Production Example 1 except that the prepolymer U1 solution (concentration: 50 mass %) was changed to the prepolymer U2 (concentration: 50 mass %).

[0256] [Measurement and Evaluation of Adhesive Sheet]

[0257] The following various evaluations were performed on the PSA sheet S1 obtained in Production Example 1 (Example 1), the commercially available PSA sheets (with release liner) S2 to S5 (Examples 2 to 5) described below, and the PSA sheet S6 (Example 6) obtained in Production Example 2. The evaluation results are shown in Table 2. It should be noted that Example 1 is an example, and Examples 2 to 6 are comparative examples.

[0258] (Adhesive Sheet)

[0259] ·S2: "Easy-to-peel silicone tape", manufactured by 3M Japan Limited, silicone-based adhesive, support: polyester nonwoven fabric

[0260] ·S3: "Single-sided adhesive tape 2476P", manufactured by 3M Japan Limited, silicone adhesive, support: polyester nonwoven fabric

[0261] ·S4: "Skin patch tape 4076", manufactured by 3M Japan Limited, acrylic adhesive, support: polyester nonwoven fabric

[0262] ·S5: "Ukiyo (registered trademark)", manufactured by Nitoms, Inc., acrylic adhesive, support: polyester nonwoven fabric

[0263] <Adhesion>

[0264] (1) Phenolic resin board

[0265] The adhesive layer side of the adhesive sheet (100 mm in length and 15 mm in width) from which the release liner was peeled off was overlapped with a phenolic resin plate ("SUMILITE (registered trademark) PL-1102", manufactured by Sumitomo Bakelite Co., Ltd.; 125 mm in length, 30 mm in width, and 2 mm in thickness), and a rubber roller was moved back and forth once from the support side of the adhesive sheet at a load of 2 kg and a speed of 300 mm / min to press the adhesive layer onto the phenolic resin plate.

[0266] After leaving the sheet to stand for 20 minutes, the pressure-sensitive adhesive sheet was peeled off at a peeling angle of 90° and a speed of 300 mm / min, and the pressure-sensitive adhesive strength was measured by a method in accordance with JIS Z 0237:2009.

[0267] Table 2 also shows the evaluation of the measured adhesive strength based on the following evaluation criteria.

[0268] 〔Evaluation criteria (phenolic resin board)〕

[0269] A: 3.0N / 15mm or more

[0270] B: 2.0N / 15mm or more and less than 3.0N / 15mm

[0271] C: less than 2.0N / 15mm

[0272] If the evaluation is A, it can be said that the film has good adhesion to phenol resin which is a typical material such as a sealing material for a circuit pattern.

[0273] (2) To human skin

[0274] The adhesive strength was similarly measured when the skin of the forearm of a human (subject) was used as an adherend instead of the phenolic resin plate. The average value of the three measured values ​​is shown in Table 2. In addition, in Example 6, the adhesive was not adhered to the skin.

[0275] Table 2 also shows the evaluation of the measured adhesive strength based on the following evaluation criteria.

[0276] 〔Evaluation Criteria (Skin)〕

[0277] A: 0.2~1.0N / 15mm

[0278] B: more than 1.0N / 15mm

[0279] C: less than 0.2N / 15mm

[0280] If the evaluation is A, it can be said that it has moderate adhesion to the skin. If it is evaluated as B, the adhesion is too strong and it is difficult to peel off, and there is a concern of pain during peeling. If it is evaluated as C, the adhesion is too weak and it is easy to peel off or it does not adhere.

[0281] <Amount of exfoliation>

[0282] In the measurement of the adhesive strength (2), a sample of 20 mm in length and 15 mm in width was cut out from the adhesive sheet peeled off from the skin, and the amount of keratin peeling (protein amount [mg / cm 2 ]).

[0283] Table 2 also shows the evaluation of the keratin peeling amount based on the following evaluation criteria.

[0284] [Evaluation Criteria]

[0285] A: Less than 0.1 mg / cm 2

[0286] B: 0.1mg / cm 2 More than and less than 0.3 mg / cm 2

[0287] C: 0.3mg / cm 2 above

[0288] When the evaluation is A, it can be said that the load on the skin of the adhesive layer is sufficiently small.

[0289] <Long-term adhesion>

[0290] The same operation as in the above-mentioned measurement of adhesive strength (2) was performed, and the adhesive sheet was pressed against the skin of the forearm of a person (subject), and the subject spent a maximum of 14 days of daily life (working, showering, sleeping, etc.) in this state. The number of days until the adhesive sheet was peeled off (sustainability) was measured, and the presence of skin abnormalities (redness, itching, etc.) during peeling (in the case of 14 days of continuous attachment, the angle between the skin of the forearm and the adhesive sheet was maintained at 90°) was confirmed.

[0291] <Moisture Permeability>

[0292] The moisture permeability of the adhesive sheet from which the release liner was peeled off was measured by the method according to JIS Z0208: 1976. Specifically, a cup containing about 50 g of a moisture absorbent (calcium chloride) was covered with a circular adhesive sheet having a diameter of about 10 mm larger than the inner diameter of the cup, and the test piece was screwed in place using a rubber seal and a ring, and the test was performed in a constant temperature and humidity chamber at 40°C and 90% RH. The moisture permeability was calculated according to the following formula.

[0293] Moisture permeability [g / (m 2 ·day)]=W×240000 / S

[0294] Where S represents the area of ​​the opening of the cup (moisture permeable area [cm 2 ]), W represents the mass increase of the test piece per hour [g / hr].

[0295] Table 2 also shows the evaluation of the moisture permeability based on the following evaluation criteria.

[0296] [Evaluation Criteria]

[0297] A: 1500g / (m 2 ·day) or more

[0298] B: 1000g / (m 2 ·day) and less than 1500g / (m 2 ·day)

[0299] C: less than 1000g / (m 2 ·day)

[0300] If the evaluation is A, it can be said that the moisture permeability is good and the load on the skin is very small.

[0301] In addition, the moisture permeability of only the adhesive layer of the adhesive sheet S1 was measured as follows.

[0302] In Production Example 1, a PSA sheet was produced in the same manner as in Production Example 1, except that a coarse mesh nylon net which was considered not to affect the moisture permeability (without a support) was used instead of the polyester nonwoven fabric as a support. The moisture permeability of a test piece (considered to have no support) obtained by peeling off the release liner from the obtained PSA sheet was measured in the same manner as the measurement of the moisture permeability of the above-mentioned PSA sheet, and the measured value was regarded as the moisture permeability of only the PSA layer.

[0303] As a result, the moisture permeability of only the adhesive layer of the adhesive sheet S1 was 4900 g / (m 2 ·day).

[0304] [Table 2]

[0305] Table 2

[0306]

[0307] [Manufacturing of bonded circuits]

[0308] (Example 7)

[0309] In Production Example 1, the dry film thickness of the adhesive layer was set to 100 μm, and a polyurethane film (thickness 20 μm) was bonded as a support onto the obtained adhesive layer. The same operation as in Production Example 1 was carried out to produce an adhesive sheet S7.

[0310] A sheet piece (20 mm in length and 70 mm in width) was cut out from the adhesive sheet S7, and a circuit was formed on the support side by screen printing using a silver paste, and dried at 70 to 80° C. for 30 minutes to obtain a bonded circuit.

[0311] (Examples 8, 9)

[0312] Using the adhesive sheets S3 and S5, the same operation as in Example 7 was carried out to produce a bonded circuit.

[0313] [Evaluation of Attached Circuit]

[0314] The circuit retention properties were evaluated for the attached circuits of Examples 7 to 9. The evaluation results are shown in Table 3. It should be noted that Example 7 is an example, and Examples 8 and 9 are comparative examples.

[0315] <Circuit Retention>

[0316] The attached circuit was pressed against the skin of the forearm of a person (subject) in the same manner as in the measurement of the adhesive strength of the adhesive sheet (2), and the subject spent one day of daily life in this state (except for showering). The presence or absence of peeling of the circuit and the presence or absence of discoloration at the interface between the circuit and the support were checked. The discoloration was considered to be mainly due to corrosion of the circuit.

[0317] [Table 3]

[0318] Table 3

[0319]

[0320] According to the evaluation results shown in Tables 2 and 3, it is believed that the adhesive sheets (S1, S7) manufactured using prepolymer U1 (hydroxy-terminated urethane prepolymer) have excellent moisture permeability even if they are adhesive sheets with a support, suppress the load on the skin, and show moderate adhesive strength. In addition, they also have excellent adhesion to electronic devices, etc., and can suppress circuit peeling or circuit operation defects caused by corrosion.

[0321] Description of Reference Numerals

[0322] 11 Adhesive layer

[0323] 12 Support

[0324] 21 Circuit Pattern

[0325] 22 substrate (package)

[0326] 23 Insulation layer

[0327] 31 Other adhesive layers

[0328] 40 Skin

Claims

1. A bonding circuit having a circuit pattern and an adhesive layer, The adhesive constituting the adhesive layer comprises a reaction product of a hydroxyl-terminated urethane prepolymer and a curing agent. The hydroxyl-terminated urethane prepolymer is a reaction product of an oxyalkylene polymer A having an average hydroxyl number of 2.1 to 3.0 per molecule, an oxyalkylene polymer B having a hydroxyl number of 1 per molecule, and a diisocyanate compound, and the content of ethylene oxide units is 5% by mass or more. The curing agent includes a polyisocyanate compound.

2. The attached circuit according to claim 1, wherein: The number average molecular weight of the oxyalkylene polymer B is 3,500 or more.

3. The attached circuit according to claim 1 or 2, wherein: In a total of 100 parts by mass of the oxyalkylene polymer A, the amount of the oxyalkylene polymer A1 having 3 hydroxyl groups per molecule is 20 parts by mass or more.

4. The attached circuit according to any one of claims 1 to 3, wherein: The content of ethylene oxide units in the oxyalkylene polymer A is 10% by mass or more.

5. The attached circuit according to any one of claims 1 to 4, wherein: The amount of polymer A to be added is 10 to 95 parts by mass based on 100 parts by mass of the total of polymer A and polymer B.

6. The attached circuit according to any one of claims 1 to 5, wherein: The polyisocyanate compound has three or more isocyanate groups in one molecule.

7. The attached circuit according to any one of claims 1 to 6, wherein: The thickness of the adhesive layer is 5 to 100 μm.

8. The attached circuit according to any one of claims 1 to 7, wherein: The moisture permeability of the adhesive layer is 3000 g / (m 2 ·day) or more.

9. The attached circuit according to any one of claims 1 to 8, wherein: The adhesive layer is formed on a main surface of a sheet-like support.

10. The attached circuit according to claim 9, wherein: The adhesive layer is formed on one main surface of the support, and the circuit pattern is formed on the other main surface of the support.

11. The attached circuit according to any one of claims 1 to 10, wherein: The circuit pattern is formed of conductive ink. 12 . A wearable device comprising the patch circuit according to claim 1 .