Wiring substrate, method for manufacturing same, and semiconductor device

By adjusting the arithmetic average roughness on the electrode pad connection surface, the cracking problem caused by thermal stress of the insulating resin layer of the wiring substrate is solved, and high insulation reliability is achieved, and it is suitable for the fine wiring environment of semiconductor devices.

CN118975415APending Publication Date: 2024-11-15RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094498.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the wiring substrate, cracks occur between the insulating resin layer and the wiring layer due to thermal stress, which affects its high insulation reliability.

Method used

By processing on the connection surface of the electrode pad, the arithmetic average roughness is 0.5 μm or more and 2.0 μm or less, thereby forming a surface that improves adhesion and reduces defects, thereby suppressing defect generation of the insulating resin layer.

Benefits of technology

The defects of the insulating resin layer caused by temperature changes are effectively suppressed, and the high insulation reliability of the semiconductor device is ensured, especially in the case of fine wiring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118975415A_ABST
    Figure CN118975415A_ABST
Patent Text Reader

Abstract

A wiring board includes a wiring portion including a wiring layer, and an electrode pad provided on the wiring portion and connected to the wiring layer. A connection surface, which is a surface on the opposite side of the electrode pad from the wiring portion, has an arithmetic average roughness Ra of 0.5 [mu] m or more and 2.0 [mu] m or less. The wiring substrate may further have a surface insulating resin layer provided on the surface of the wiring portion on the electrode pad side and having an opening through which the electrode pad is exposed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a wiring substrate, a connection method thereof, and a semiconductor device. Background Art

[0002] In a wiring substrate having a wiring layer and an insulating layer, cracks may occur at the interface between the wiring layer and the insulating layer due to thermal stress caused by mounting of a semiconductor chip or the like (for example, Patent Document 1).

[0003] Previous technical literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-157666 Summary of the invention

[0006] Technical issues to be solved by the invention

[0007] One aspect of the present invention relates to a wiring substrate having an electrode pad exposed in an opening of an insulating resin layer, and to suppressing the occurrence of defects in the insulating resin layer due to temperature changes.

[0008] Means for solving technical problems

[0009] One aspect of the present invention relates to a wiring substrate, comprising a wiring portion including a wiring layer and an electrode pad provided on the wiring portion and connected to the wiring layer, wherein a surface of the electrode pad opposite to the wiring portion, i.e., a connection surface, has an arithmetic mean roughness Ra of not less than 0.5 μm and not more than 2.0 μm.

[0010] Another aspect of the present invention relates to a semiconductor device including the above-mentioned wiring substrate and a semiconductor chip mounted on the wiring substrate.

[0011] Another aspect of the present invention relates to a method for manufacturing a wiring substrate, which includes the following steps: preparing a wiring structure, the wiring structure having a wiring portion including a wiring layer and an electrode pad arranged on the wiring portion; and treating the surface of the electrode pad on the opposite side of the wiring portion, i.e., the connection surface, so as to have an arithmetic mean roughness Ra of greater than 0.5 μm and less than 2.0 μm.

[0012] Effects of the Invention

[0013] The wiring substrate having the electrode pad exposed in the opening of the insulating resin layer can suppress the occurrence of defects on the insulating resin layer due to temperature changes. Therefore, even when the semiconductor device has fine wiring, high insulation reliability can be easily maintained. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a process diagram showing an example of a method for manufacturing a wiring board.

[0015] Figure 2 This is a process diagram showing an example of a method for manufacturing a wiring board.

[0016] Figure 3 is a cross-sectional view showing an example of a semiconductor device. DETAILED DESCRIPTION

[0017] The present invention is not limited to the following examples. In the following description, the same symbols are sometimes marked for the same or equivalent parts, and repeated descriptions are omitted. Unless otherwise specified, the positional relationship such as up, down, left, and right is based on the positional relationship shown in the drawings. The dimensional ratios of the accompanying drawings are not limited to the ratios shown in the drawings. Terms such as "left", "right", "front", "back", "up", "down", "above", and "below" do not necessarily mean that their relative positions remain unchanged. The term "layer" also includes structures formed in a part of the shape in addition to structures formed in the shape of the entire surface when observed as a top view.

[0018] Figure 1 and Figure 2 This is a process diagram showing an example of a method for manufacturing a wiring board. Figure 1 and Figure 2 The method shown may include the following steps: preparing a wiring substrate 10 (wiring structure), the wiring substrate 10 including a base material 1, a wiring section 3 provided on the base material 1, and an electrode pad 5 provided on the surface of the wiring section 3 on the side opposite to the base material 1; and treating the surface of the electrode pad 5 on the side opposite to the wiring section 3, that is, the connection surface 5S, so as to have an arithmetic mean roughness Ra of 0.5 μm or more and 2.0 μm or less. In this specification, the wiring substrate before the connection surface is treated is sometimes referred to as a wiring structure.

[0019] The process of preparing wiring board 10 includes forming wiring section 3 including an insulating resin layer and a wiring layer on a main surface of base material 1 and forming electrode pads 5 on a surface of wiring section 3 opposite to base material 1 .

[0020] The substrate 1 may be, for example, a silicon substrate, a glass substrate, a stainless steel substrate, or a glass cloth, or may be a semiconductor package having a semiconductor chip and a sealing resin layer sealing the semiconductor chip.

[0021] The thickness of the substrate 1 can be, for example, 0.2 mm or more and 2.0 mm or less. A substrate having a thickness of 0.2 mm or more is easy to have good handling properties. From the perspective of manufacturing cost, a substrate having a thickness of 2.0 mm or less is generally advantageous. The substrate 1 can be a wafer having a circular main surface or a panel having a rectangular main surface. For example, the substrate 1 can be a wafer having a circular main surface with a diameter of 200 mm or more and 450 mm or less, or a panel having a rectangular main surface with a width of 300 mm or more and 700 mm or less.

[0022] The wiring section 3 can be formed by a method including forming an insulating resin layer and a wiring layer provided in the insulating resin layer by a common method. The wiring section 3 may have a multilayer wiring structure including two or more wiring layers.

[0023] The electrode pad 5 can include, for example, the following steps: forming a seed layer on the surface of the wiring portion 3 on the opposite side of the substrate 1; forming a resist layer 4 having an opening 4a exposing a portion of the seed layer on the seed layer; forming an electrode pad 5 including an electrolytic plating layer filling the opening 4a; removing the resist layer 4; and removing the portion of the seed layer not covered by the electrolytic plating layer. The method for forming the seed layer may include the following steps: cleaning the surface of the wiring portion 3 with a pretreatment solution; and adsorbing a palladium catalyst on the surface of the wiring portion 3. The seed layer can also be formed by sputtering. The seed layer can be a metal layer containing a metal species such as copper or titanium. The thickness of the seed layer can be greater than 20nm and less than 200nm, greater than 40nm and less than 200nm, or greater than 60nm and less than 200nm.

[0024] The electrode pad 5 may be a copper pad containing copper. The thickness of the electrode pad 5 may be 1 μm or more and 20 μm or less, 3 μm or more and 15 μm or less, or 5 μm or more and 15 μm or less.

[0025] The shape of the connection surface 5S of the electrode pad 5 or the opening 4a for forming the connection surface may be circular or elliptical. The maximum width of the electrode pad 5 (connection surface 5S) and the opening 4a may be 5 μm or more or 20 μm or more, or may be 400 μm or less, 300 μm or less, or 10 μm or less. The electrode pad 5 (connection surface 5S) and the opening 4a may have an area equivalent to the area of ​​a circle having a diameter of 5 μm or more and 400 μm or less, or 5 μm or more and 10 μm or less.

[0026] The connection surface 5S in the prepared wiring substrate 10 is processed so as to have an arithmetic mean roughness Ra of 0.5 μm or more and 2.0 μm or less. From the viewpoint of improving the adhesion based on the anchoring effect, a large arithmetic mean roughness Ra is advantageous, but according to the understanding of the present inventors, if the arithmetic mean roughness Ra exceeds 2.0 μm, defects such as cracks are likely to occur on the insulating resin layer (especially the surface insulating resin layer 7 described later) in contact with the connection surface 5S. The arithmetic mean roughness Ra can be measured by a method according to JIS B0601-1994.

[0027] In the case where the connection surface 5S before the treatment has an arithmetic mean roughness Ra of less than 0.5 μm, the connection surface 5S is roughened in such a way that the arithmetic mean roughness Ra becomes greater than 0.5 μm and less than 2.0 μm. In the case where the connection surface 5S before the treatment has an arithmetic mean roughness Ra of more than 2.0 μm, the connection surface 5S is smoothed in such a way that the arithmetic mean roughness Ra becomes greater than 0.5 μm and less than 2.0 μm. The roughening treatment and the smoothing treatment may include a process of contacting the connection surface 5S with a treatment liquid. The treatment liquid used for the roughening treatment may be, for example, an acidic aqueous solution. The acidic aqueous solution may contain an organic acid or an inorganic acid, a copper ion source, a halide ion source and a polymer. The organic acid may be, for example, formic acid, acetic acid, propionic acid, butyric acid or a combination thereof. The inorganic acid may be, for example, sulfuric acid, hydrochloric acid or a combination thereof. The halide may be, for example, hydrochloric acid, hydrobromic acid, sodium chloride, potassium chloride, calcium chloride, potassium bromide or a combination thereof. The copper ion source may be, for example, copper chloride, copper bromide, copper hydroxide, copper oxide, or a combination thereof. The polymer may have a polyamine chain or a cationic group (e.g., a quaternary ammonium group). The treatment liquid for smoothing treatment may be selected from, for example, the following treatment liquids: a treatment liquid containing an imidazole compound and a sugar alcohol; a treatment liquid containing an aromatic compound having an amino group and an aromatic ring, a polyacid, and a halide ion or an oxidant (hypochlorous acid, chlorous acid, chloric acid, perchloric acid, persulfuric acid, percarbonic acid, hydrogen peroxide, organic peroxide, etc.); a treatment liquid containing an aromatic compound having an amino group and an aromatic ring and a sulfur compound; and a treatment liquid containing a silane coupling agent, a metal ion, and a halide ion.

[0028] On the processed connection surface 5S, the number of protrusions with a height exceeding 3 μm may be 5 or less per 15 μm of length in the in-plane direction of the connection surface 5S. A relatively large protrusion with a height exceeding 3 μm may become a starting point for defects such as cracks on the surface insulating resin layer. The height of the protrusion is the height of the deeper side of the bottom of the concave portion on both sides of the protrusion when measuring the concavity and convexity of the connection surface 5S along the in-plane direction of the connection surface 5S. The number of protrusions with a height exceeding 3 μm may be 4 or less, 3 or less, 2 or less, or 1 or less per 15 μm of length in the in-plane direction of the connection surface 5S.

[0029] After the connection surface 5S is processed, a surface insulating resin layer 7 is formed which is provided on the surface of the wiring portion 3 on the side opposite to the substrate 1 and has an opening 7a exposing the central portion of the electrode pad 5. The surface insulating resin layer 7 is formed so as to be in contact with the peripheral portion of the connection surface 5S. The thickness of the portion of the surface insulating resin layer 7 in contact with the wiring portion 3 may be 15 μm or more and 30 μm or less.

[0030] The surface insulating resin layer 7 can be formed of a resist material commonly used to form a solder resist, for example. The opening 7a can be formed, for example, by laser ablation, photolithography (exposure and development), or imprinting. The material used to form the surface insulating resin layer 7 can be a thermosetting or photocurable resist material. In the case of photolithography, a photocurable resist material is used.

[0031] The thermosetting resist material may include a thermosetting resin that is cured by heating to form a cured product showing electrical insulation. The thermosetting resin may be, for example, an epoxy resin, a phenolic resin, a resin containing a triazine ring, an unsaturated polyester resin, a bismaleimide resin, a diallyl phthalate resin, a silicone resin, a resin having a benzoxazine ring, a norbornene resin, a cyanate resin, an isocyanate resin, an urethane resin, a benzocyclobutene resin, a maleimide resin, a bismaleimide triazine resin, a polyazomethine resin, a thermosetting polyimide, or a combination thereof. Examples of epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, bisphenol E epoxy resins, bisphenol M epoxy resins, bisphenol P epoxy resins, and bisphenol Z epoxy resins; bisphenol A novolac epoxy resins, phenol novolac epoxy resins, and cresol novolac epoxy resins; novolac epoxy resins; biphenyl epoxy resins, biphenyl aralkyl epoxy resins, arylalkyl epoxy resins, tetraphenol ethane epoxy resins, naphthalene epoxy resins, anthracene epoxy resins, phenoxy epoxy resins, dicyclopentadiene epoxy resins, norbornene epoxy resins, and the like. Type epoxy resin, adamantane type epoxy resin, fluorene type epoxy resin, methacrylate glycidyl copolymer epoxy resin, copolymer of cyclohexylmaleimide and methacrylate glycidyl, epoxy-modified polybutadiene rubber derivative, CTBN modified epoxy resin, trimethylolpropane polyglycidyl ether, phenyl-1,3-diglycidyl ether, biphenyl-4,4'-diglycidyl ether, 1,6-hexanediol diglycidyl ether, diglycidyl ether of ethylene glycol or propylene glycol, sorbitol polyglycidyl ether, tri(2,3-epoxypropyl) isocyanurate and triglycidyl tri(2-hydroxyethyl) isocyanurate. Examples of phenolic resins include novolac-type phenolic resins such as phenol novolac resins, cresol novolac resins, and bisphenol A novolac resins, and m-cresol-type phenolic resins such as unmodified m-cresol novolac resins and oil-modified m-cresol novolac resins modified with tung oil, linseed oil, or walnut oil. Examples of triazine ring-containing resins include urea resins and melamine resins.

[0032] The photocurable resist material may contain, for example, an epoxy resin (alicyclic epoxy resin, etc.), an oxetane compound, a vinyl ether compound, or a photocurable resin which is a combination thereof. Examples of the alicyclic epoxy resin include 3,4,3',4'-diepoxybiscyclohexane, 2,2-bis(3,4-epoxycyclohexyl)propane, 2,2-bis(3,4-epoxycyclohexyl)-1,3-hexafluoropropane, bis(3,4-epoxycyclohexyl)methane, 1-[1,1-bis(3,4-epoxycyclohexyl)]ethylbenzene, bis(3,4-epoxycyclohexyl)adipate, 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate, (3,4-epoxy-6-methylcyclohexyl)methyl-3',4'-epoxy-6-methylcyclohexanecarboxylate, ethylene-1,2-bis(3,4-epoxycyclohexanecarboxylate), cyclohexene oxide, 3,4-epoxycyclohexylmethanol, and 3,4-epoxycyclohexylethyltrimethoxysilane.

[0033] The material for forming the surface insulating resin layer 7 can include thermoplastic resin. Thermoplastic resin can be general-purpose plastic, engineering plastic, thermoplastic elastomer or their combination. As the example of general-purpose plastic, acrylic resin, modified acrylic resin, low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, polyethylene terephthalate, polypropylene, modified polypropylene, polystyrene, acrylonitrile-butadiene-styrene copolymer, acrylonitrile-styrene copolymer, cellulose acetate, polyvinyl alcohol, polyvinyl chloride, polyvinylidene chloride and polylactic acid can be enumerated. As the example of engineering plastic, polyamide, thermoplastic polyurethane, polyacetal, polycarbonate, ultra-high molecular weight polyethylene, polybutylene terephthalate, modified polyphenylene ether, polysulfone, polyphenylene sulfide, polyether sulfone, polyether ether ketone, polyarylate, polyetherimide, polyamide-imide, liquid crystal polymer, polyamide 6T, polyamide 9T, polytetrafluoroethylene, polyvinylidene fluoride, polyesterimide and thermoplastic polyimide can be enumerated. Examples of the thermoplastic elastomer include olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, polyester-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, amide-based thermoplastic elastomers, vinyl chloride-based thermoplastic elastomers, and hydrogenated thermoplastic elastomers.

[0034] The material used to form the surface insulating resin layer 7 may include an inorganic filler. The inorganic filler can help improve the reliability and rigidity of the surface insulating resin layer 7. The inorganic filler may be, for example, silicon dioxide, barium sulfate, barium titanate, talc, clay, calcined kaolin, magnesium carbonate, calcium carbonate, aluminum oxide, aluminum hydroxide, mica powder, or a combination thereof.

[0035] A semiconductor device can be obtained by mounting a semiconductor chip on the wiring board obtained by the above method. Figure 3is a cross-sectional view showing an example of a semiconductor device. Figure 3 The semiconductor device 100 shown includes: a wiring substrate 10; a semiconductor chip 20 mounted on the wiring substrate 10; a solder bump 25 between the semiconductor chip 20 and the electrode pad 5 of the wiring substrate 10 and electrically connecting them; and an insulating resin layer 30 (adhesive layer) filled between the semiconductor chip 20 and the wiring substrate 10.

[0036] In a semiconductor device having fine wiring and a plurality of pins, the generation of cracks on the insulating resin layer can also be effectively suppressed. The semiconductor device may have an insert including a fine wiring layer for mixed loading of different types of semiconductor chips. For example, the interval between the pins provided on the semiconductor chip may be less than 200 μm or less than 100 μm, or may be more than 30 μm. The number of pins provided on the semiconductor chip may be more than 500 or more than 1,000, or may be less than 10,000.

[0037] Example

[0038] The present invention is not limited to the following examples.

[0039] A wiring substrate was prepared, wherein the wiring substrate had a copper pad having a connection surface (width 260 μm) with an arithmetic mean roughness Ra of 0.03 μm and a surface insulating resin layer (solder resist) having an opening exposing the copper pad. The connection surface of the copper pad was roughened by a roughening treatment liquid to form a surface with an arithmetic mean roughness Ra of 0.5 μm, 1.0 μm, 2.0 μm, 3.0 μm or 5.0 μm. The arithmetic mean roughness Ra was measured using a laser microscope (manufactured by Olympus Corporation, OLS4100). A semiconductor chip was mounted on the wiring substrate using a nitrogen reflow oven in a manner connected to the treated connection surface via a solder bump. The temperature of the nitrogen reflow oven was set to 260°C. It was confirmed that the solder bump and the semiconductor chip were connected to the wiring substrate, and the insulating resin layer was filled between the semiconductor chip and the wiring substrate and thermally cured. The formed semiconductor device was placed in a temperature cycle tester and subjected to 400 cycles of heat treatment under the conditions of 165° C. on the high temperature side, −65° C. on the low temperature side, and a holding time of 15 minutes.

[0040] The cross section of the surface insulating resin layer adjacent to the copper pad in the semiconductor device subjected to the heat treatment was observed to confirm the presence or absence of cracks. The results are shown in Table 1. By forming a connection surface with an Ra of 0.5 μm or more and 2.0 μm or less, it was confirmed that the generation of cracks on the surface insulating resin layer was effectively suppressed. In the case of Ra of 0.03 μm, interface peeling was observed between the connection surface and the surface insulating resin layer, suggesting insufficient adhesion.

[0041] [Table 1]

[0042]

[0043] Explanation of symbols

[0044] 3-wiring portion, 4a, 7a-openings, 5-electrode pads, 5S-connection surface, 7-surface insulating resin layer, 10-wiring substrate (wiring structure), 20-semiconductor chip, 25-solder bumps, 100-semiconductor device.

Claims

1. A wiring substrate comprising: a wiring section, including a wiring layer; and an electrode pad, which is disposed on the wiring portion and connected to the wiring layer, The surface of the electrode pad on the opposite side to the wiring portion, ie, the connection surface, has an arithmetic mean roughness Ra of 0.5 μm or more and 2.0 μm or less.

2. The wiring substrate according to claim 1, in, The number of protrusions on the connection surface having a height exceeding 3 μm is 5 or less per 15 μm of the length in the in-plane direction of the connection surface.

3. The wiring substrate according to claim 1 or 2, in, The wiring substrate further includes a surface insulating resin layer provided on the surface of the wiring portion on the electrode pad side and having an opening exposing the electrode pad. The surface insulating resin layer is in contact with a portion of the connection surface.

4. The wiring substrate according to claim 3, in, The surface insulating resin layer is a layer formed of a thermosetting or photocurable resist material containing an epoxy resin.

5. A semiconductor device comprising: The wiring substrate according to any one of claims 1 to 4; and A semiconductor chip is mounted on the wiring substrate.

6. A method for manufacturing a wiring substrate, comprising the following steps: preparing a wiring structure including a wiring portion including a wiring layer and an electrode pad provided on the wiring portion; and The surface of the electrode pad on the opposite side to the wiring portion, ie, the connection surface, is processed to have an arithmetic mean roughness Ra of 0.5 μm or more and 2.0 μm or less.

7. The method according to claim 6, in, The connection surface is processed to have an arithmetic mean roughness Ra of 0.5 μm or more and 2.0 μm or less and to have 5 or less protrusions having a height exceeding 3 μm per 15 μm of the length in the in-plane direction of the connection surface.

8. The method according to claim 6 or 7, in, The method further includes the step of forming a surface insulating resin layer on the surface of the wiring portion on the electrode pad side, the surface insulating resin layer having an opening exposing the connection surface, The surface insulating resin layer is formed so as to be in contact with a portion of the connection surface.

9. The method according to claim 8, in, The surface insulating resin layer is formed of a thermosetting or photocurable resist material including an epoxy resin.