A high-purity viscose-based carbon fiber composite material graphite felt and its preparation process
By modifying viscose fiber needle-punched felt with butanetetracarboxylic acid and copper doping, combined with in-situ reduction reaction of copper sulfate and low-temperature carbonization process, the problems of cracking and poor thermal conductivity of viscose-based graphite felt were solved, and the excellent thermal conductivity and crack resistance of high-purity viscose-based carbon fiber composite graphite felt were achieved.
Patent Information
- Application Number
- CN202411082047.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Viscose-based graphite felt is prone to cracking during the preparation process and has poor thermal conductivity, which affects the battery's lifespan and performance.
Modified viscose fiber needle-punched felt is used. Through butanetetracarboxylic acid modification and copper doping, combined with the in-situ reduction reaction of copper sulfate and coupling with 3-aminopropyltrihydroxysilane, a multi-component cross-linked network structure is formed, which increases the copper loading and bond content. Combined with the low-temperature carbonization and high-temperature carbonization process, the thermal conductivity and crack resistance are enhanced.
It significantly improves the thermal conductivity and crack resistance of graphite felt, reduces the possibility of defect structure formation during pyrolysis, and enhances the overall performance of the battery.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of functional battery electrode materials, and more specifically, to a high-purity viscose-based carbon fiber composite material graphite felt and a preparation process thereof. Background Art
[0002] Electrode is one of the main components of RFE, and due to the common presence of corrosive liquid in RFE, there are fewer electrode materials available. Graphite felt has a wide working potential range, and it is also corrosion-resistant, highly conductive, and low-cost, so it is one of the relatively superior electrode materials in RFE.
[0003] Graphite felt can be divided into three types according to the material: asphalt-based graphite felt, polyacrylonitrile-based graphite felt and viscose-based graphite felt. Among them, viscose-based graphite felt has the advantages of good flexibility and low volume density. However, at the same time, viscose-based graphite felt is prone to cracking due to high temperature during the preparation process. At the same time, when viscose-based graphite felt is actually used, due to its poor thermal conductivity, it is likely to cause heat accumulation inside the battery, thereby affecting the battery life and performance.
[0004] Therefore, there is an urgent need for a viscose-based graphite felt material having both excellent mechanical strength and excellent thermal conductivity. Summary of the invention
[0005] In order to improve the defects of conventional viscose-based graphite felt materials, that is, their mechanical properties and thermal conductivity are relatively poor, the present application provides a high-purity viscose-based carbon fiber composite material graphite felt and a preparation process thereof.
[0006] In the first aspect, the present application provides a high-purity viscose-based carbon fiber composite material graphite felt, which adopts the following technical solution:
[0007] A high-purity viscose-based carbon fiber composite material graphite felt, wherein the high-purity viscose-based carbon fiber composite material graphite felt is prepared by pre-oxidation, carbonization and graphitization of modified viscose fiber needle-punched felt;
[0008] The modified viscose fiber needle-punched felt is prepared by a needle-punching process of copper-doped viscose fiber modified with butanetetracarboxylic acid, and the copper of the copper-doped viscose fiber contains hydroxyl groups.
[0009] The reason why graphite has poor thermal conductivity is that it is not uniform enough. Its thermal conductivity is extremely high in the direction parallel to the plane, but relatively low in the direction perpendicular to the plane. Although copper is inferior to graphite in terms of maximum thermal conductivity, it has better uniformity. Therefore, after copper is doped on viscose fiber, graphite felt will have better thermal conductivity overall in the pre-oxidation, carbonization and graphitization processes.
[0010] However, the dispersion of copper and viscose fiber is very poor, and it is difficult for copper to effectively connect with viscose fiber, which leads to a relatively small amount of copper on viscose fiber. In addition, the reason for the cracks in graphite felt is that during the pyrolysis of viscose fiber, viscose fiber will produce a large number of complex reactions, which will cause a large number of defective structures in the graphite felt itself, and the scattered copper will cause the defective structures to increase further, and these defective structures are one of the reasons for the cracks in graphite felt.
[0011] After modification with butanetetracarboxylic acid, the two adjacent carboxyl groups of butanetetracarboxylic acid are first dehydrated into anhydrides, and then the highly active cyclic anhydrides further react with the hydroxyl groups on the viscose fiber macromolecules to form esters and release a carboxyl group. The released carboxyl group can also be dehydrated with another adjacent carboxyl group to form anhydrides and connect with another hydroxyl group on the viscose fiber. At the same time, the remaining carboxyl groups can also connect with the hydroxyl groups on copper, thereby forming a multi-crosslinked network structure. While effectively increasing the copper loading of the viscose fiber, it can also effectively increase the bond content in the viscose fiber, thereby inhibiting the generation of defects during the pyrolysis process and effectively reducing the possibility of cracks in the graphite felt.
[0012] Preferably, the preparation method of the copper-doped viscose fiber is: soaking the viscose fiber in a penetrant JFC solution, treating it at a temperature of 30-40° C. for 10-30 minutes, then washing and drying it, and then putting it into a copper sulfate solution, shaking it for reaction, then washing it, soaking it again in 3-aminopropyltrihydroxysilane, and finally drying it to obtain the copper-doped viscose fiber;
[0013] The mass ratio of the viscose fiber to the penetrant JFC solution is 1:(100-120), and the content of JFC in the penetrant JFC solution is 1-3%.
[0014] The dispersion of copper and viscose fiber is extremely poor, and it is difficult for copper to effectively connect with viscose fiber, which leads to a relatively small amount of copper on viscose fiber. In this application, the potential reducing groups in viscose fiber are firstly utilized to promote the accumulation of copper in the viscose fiber cavity through the in-situ reduction reaction of copper sulfate, thereby forming aggregates or even microcrystalline structures. After the reaction, the pores of the viscose fiber shrink, and copper is deposited in the viscose fiber cavity, which effectively limits the shedding of copper, thereby increasing the copper loading of the graphite felt, and at the same time prepares for the subsequent 3-aminopropyltrihydroxysilane coupling and butanetetracarboxylic acid, effectively improving the thermal conductivity and crack resistance of the high-purity viscose-based carbon fiber composite material graphite felt.
[0015] Preferably, the concentration of the copper sulfate solution is 3.5-4.5 mmol / L, the oscillation reaction temperature is 85-95° C., and the oscillation reaction time is 90-150 min.
[0016] When copper sulfate adopts the above concentration and the above reaction temperature and reaction time are selected, a higher copper loading will be obtained on the graphite felt, thereby effectively improving the thermal conductivity of the high-purity viscose-based carbon fiber composite material graphite felt.
[0017] Preferably, the method for preparing the copper-doped viscose fiber modified with butanetetracarboxylic acid comprises the following steps:
[0018] S1. First, soak the copper-doped viscose fiber in a sodium sulfite aqueous solution at a soaking temperature of 70-80° C. for 1-2 h, and then wash with water to obtain the pretreated copper-doped viscose fiber;
[0019] S2, performing a three-immersion and three-rolling treatment on the pretreated copper-doped viscose fiber, wherein the immersion solution contains butane tetracarboxylic acid and sodium hypophosphite, and then drying at 40-50° C. to a constant weight to obtain butane tetracarboxylic acid-copper-doped viscose fiber;
[0020] S3, transferring the butanetetracarboxylic acid-copper-doped viscose fiber to a temperature of 150-210° C. for crosslinking for 3-6 minutes, and finally washing and drying for equilibrium to obtain butanetetracarboxylic acid-modified copper-doped viscose fiber.
[0021] Preferably, in S1, the concentration of the sodium sulfite aqueous solution is 20-30 g / L, and the mass ratio of the copper-doped viscose fiber to the sodium sulfite aqueous solution is 1:(100-120).
[0022] Preferably, in S2, the mass ratio of butane tetracarboxylic acid to sodium hypophosphite is (1-2):1, the content of butane tetracarboxylic acid in the soaking solution is 5-10%, and the mass ratio of the pretreated copper-doped viscose fiber to the soaking solution is 1:(40-50).
[0023] When butanetetracarboxylic acid is added in the above amount, the prepared modified viscose fiber needle-punched felt will have a more complete and stable cross-linked network structure, thereby further inhibiting the generation of defects in the subsequent pyrolysis process and effectively reducing the possibility of cracks in the graphite felt.
[0024] In a second aspect, the present application provides a method for preparing a high-purity viscose-based carbon fiber composite material graphite felt, using the following technical solution:
[0025] A method for preparing high-purity viscose-based carbon fiber composite material graphite felt comprises the following steps:
[0026] Pre-oxidation:
[0027] Firstly, the modified viscose needle felt is sequentially passed through six different temperature zones in a nitrogen atmosphere, each temperature zone includes an upper temperature zone and a lower temperature zone, the upper surface of the modified viscose needle felt is heated and pre-oxidized in the upper temperature zone, and the lower surface of the modified viscose needle felt is heated and pre-oxidized in the lower temperature zone to obtain a pre-oxidized felt;
[0028] Carbonization:
[0029] In a nitrogen atmosphere, the preoxidized felt is carbonized at a temperature of 500-900° C. to obtain a carbonized felt;
[0030] Graphitization:
[0031] In a nitrogen atmosphere, the carbonized felt is graphitized at a temperature of 1800-2200° C. to obtain a high-purity viscose-based carbon fiber composite material graphite felt.
[0032] Preferably, in the pre-oxidation, the specific parameters of the six temperature intervals are as follows:
[0033] Zone 1: upper temperature zone 250-400℃, lower temperature zone 250-300℃, material residence time 5-10min;
[0034] Interval 2: upper temperature zone 200-300℃, lower temperature zone 200-250℃, material residence time 10-15min;
[0035] Zone 3: upper temperature zone 200-300℃, lower temperature zone 250-350℃, material residence time 20-30min;
[0036] Zone 4: upper temperature zone 150-250℃, lower temperature zone 200-280℃, material residence time 3-5min;
[0037] Zone 5: upper temperature zone 100-200℃, lower temperature zone 120-180℃, material residence time 10-20min;
[0038] Range six: upper temperature zone 100-200℃, lower temperature zone 100-150℃, material residence time 10-20min.
[0039] Preferably, in the carbonization, low-temperature carbonization is first performed at 500° C. for 2 h, and then high-temperature carbonization is performed at 900° C. for 1 h.
[0040] Preferably, in the graphitization, pre-graphitization is first performed at 1800° C. for 0.5 h, and then graphitization is performed at 2200° C. for 1 h.
[0041] In the process of carbonization or graphitization, the method of first performing low-temperature carbonization and then high-temperature carbonization or the method of first pre-graphitization and then graphitization can effectively reduce the possibility of cracks in the graphite felt. The reason may be that the low-temperature carbonization process and the pre-graphitization process can effectively slow down the generation of defective structures during the pyrolysis of viscose fibers, thereby effectively reducing the possibility of cracks in the graphite felt.
[0042] In summary, this application has the following beneficial effects:
[0043] 1. The reason why graphite has poor thermal conductivity is that it is not uniform enough. Its thermal conductivity in the direction parallel to the plane is extremely high, up to 1000-2000W / m·K, but in the direction perpendicular to the plane, its thermal conductivity is only 5-10W / m·K. Although copper is inferior to graphite in terms of maximum thermal conductivity, it has better uniformity. Therefore, after copper is doped on viscose fiber, in the pre-oxidation, carbonization and graphitization processes, the graphite felt will have better thermal conductivity overall.
[0044] 2. After the modification of butanetetracarboxylic acid, the two adjacent carboxyl groups of butanetetracarboxylic acid are first dehydrated into anhydrides, and then the cyclic anhydrides with higher activity further react with the hydroxyl groups on the viscose fiber macromolecules to form esters and release a carboxyl group. The released carboxyl group can also be dehydrated with another adjacent carboxyl group to form anhydrides and connect with another hydroxyl group on the viscose fiber. At the same time, the remaining carboxyl groups can also connect with the hydroxyl groups on copper, thereby forming a multi-crosslinked network structure. While effectively increasing the copper loading of the viscose fiber, it can also effectively increase the bond content in the viscose fiber, thereby inhibiting the generation of defects during the pyrolysis process and effectively reducing the possibility of cracks in the graphite felt.
[0045] 3. In the process of carbonization or graphitization, the method of first performing low-temperature carbonization and then high-temperature carbonization, as well as the method of first pre-graphitization and then graphitization can effectively reduce the possibility of cracks in the graphite felt. The reason may be that the low-temperature carbonization process and the pre-graphitization process can effectively slow down the generation of defective structures during the pyrolysis of viscose fibers, thereby effectively reducing the possibility of cracks in the graphite felt. DETAILED DESCRIPTION
[0046] The present application is further described in detail below in conjunction with Examples 1-7 and Comparative Examples 1-4.
[0047] raw material
[0048] Viscose fiber core is safe and healthy; penetrant JFC Haian Petrochemical; copper sulfate CAS: 7758-98-7; 3-aminopropyltrihydroxysilane CAS: 58160-99-9; butanetetracarboxylic acid CAS: 1703-58-8; sodium sulfite CAS: 7757-83-7;
[0049] Sodium hypophosphite CAS: 123333-67-5.
[0050] Example
[0051] Example 1
[0052] A high-purity viscose-based carbon fiber composite material graphite felt, which is prepared by pre-oxidation, carbonization and graphitization of modified viscose fiber needle felt;
[0053] The modified viscose fiber needle felt is made of copper-doped viscose fiber modified by butane tetracarboxylic acid through needle punching process. The specification of the modified viscose fiber needle felt is 240g / m 2 .
[0054] The preparation method of butanetetracarboxylic acid modified copper-doped viscose fiber comprises the following steps:
[0055] S1. First, the copper-doped viscose fiber is immersed in a sodium sulfite aqueous solution, the concentration of the sodium sulfite aqueous solution is 25 g / L, the mass ratio of the copper-doped viscose fiber to the sodium sulfite aqueous solution is 1:110, the immersion temperature is 75°C, the immersion time is 1.5 h, and then washed with water to obtain the pretreated copper-doped viscose fiber;
[0056] S2, the pretreated copper-doped viscose fiber is subjected to a three-immersion and three-rolling treatment, the soaking solution contains butane tetracarboxylic acid and sodium hypophosphite, the mass ratio of butane tetracarboxylic acid to sodium hypophosphite is 1.5:1, the content of butane tetracarboxylic acid in the soaking solution is 8%, the mass ratio of the pretreated copper-doped viscose fiber to the soaking solution is 1:45, and then dried at 45°C to constant weight to obtain butane tetracarboxylic acid-copper-doped viscose fiber;
[0057] S3, transferring the butanetetracarboxylic acid-copper-doped viscose fiber to a temperature of 180° C. for crosslinking for 5 minutes, and finally washing and drying for equilibrium to obtain butanetetracarboxylic acid-modified copper-doped viscose fiber.
[0058] The preparation method of copper-doped viscose fiber is as follows: soaking the viscose fiber in a penetrant JFC solution, the mass ratio of the viscose fiber to the penetrant JFC solution is 1:110, the content of JFC in the penetrant JFC solution is 2%, treating at a temperature of 35°C for 20 minutes, and then washing and drying;
[0059] Then put it into a copper sulfate solution with a mass ratio of ten times, and oscillate it. The concentration of the copper sulfate solution is 4 mmol / L, the oscillation reaction temperature is 90°C, the oscillation reaction time is 120 min, and then washed with water, immersed in excess 3-aminopropyltrihydroxysilane again, and finally taken out and dried to obtain copper-doped viscose fiber.
[0060] The preparation method of high-purity viscose-based carbon fiber composite material graphite felt comprises the following steps:
[0061] Pre-oxidation:
[0062] Firstly, the modified viscose needle felt is sequentially passed through six different temperature zones in a nitrogen atmosphere, each temperature zone includes an upper temperature zone and a lower temperature zone, the upper surface of the modified viscose needle felt is heated and pre-oxidized in the upper temperature zone, and the lower surface of the modified viscose needle felt is heated and pre-oxidized in the lower temperature zone to obtain a pre-oxidized felt;
[0063] The specific parameters of the six temperature ranges are as follows:
[0064] Zone 1: upper temperature zone 360℃, lower temperature zone 275℃, material residence time 10min;
[0065] Zone 2: upper temperature zone 275℃, lower temperature zone 210℃, material residence time 12min;
[0066] Zone 3: upper temperature zone 225℃, lower temperature zone 335℃, material residence time 25min;
[0067] Zone 4: upper temperature zone 200℃, lower temperature zone 240℃, material residence time 4min;
[0068] Zone 5: upper temperature zone 150℃, lower temperature zone 160℃, material residence time 15min;
[0069] Zone 6: upper temperature zone 150℃, lower temperature zone 120℃, material residence time 15min.
[0070] Carbonization:
[0071] In a nitrogen atmosphere, the preoxidized felt was first carbonized at 500°C for 2 h, and then carbonized at 900°C for 1 h to obtain a carbonized felt.
[0072] Graphitization:
[0073] In a nitrogen atmosphere, pre-graphitization was first carried out at 1800°C for 0.5h, and then graphitization was carried out at 2200°C for 1h to obtain high-purity viscose-based carbon fiber composite graphite felt.
[0074] Example 2
[0075] The difference from Example 1 is that in the preparation method of copper-doped viscose fiber, the concentration of the copper sulfate solution is 3.5 mmol / L, the oscillation reaction temperature is 95° C., and the oscillation reaction time is 90 min.
[0076] Example 3
[0077] The difference from Example 1 is that in the preparation method of copper-doped viscose fiber, the concentration of the copper sulfate solution is 4.5 mmol / L, the oscillation reaction temperature is 85° C., and the oscillation reaction time is 150 min.
[0078] Example 4
[0079] The difference from Example 1 is that in S2, the mass ratio of butane tetracarboxylic acid to sodium hypophosphite is 1:1, the content of butane tetracarboxylic acid in the soaking solution is 10%, and the mass ratio of the pretreated copper-doped viscose fiber to the soaking solution is 1:40.
[0080] Example 5
[0081] The difference from Example 1 is that in S2, the mass ratio of butane tetracarboxylic acid to sodium hypophosphite is 2:1, the content of butane tetracarboxylic acid in the soaking solution is 5%, and the mass ratio of the pretreated copper-doped viscose fiber to the soaking solution is 1:50.
[0082] Example 6
[0083] The difference from Example 1 is that during the carbonization, high-temperature carbonization is directly performed at 900° C. for 3 h.
[0084] Example 7
[0085] The difference from Example 1 is that during graphitization, graphitization is directly performed at a temperature of 2200° C. for 1.5 h.
[0086] Comparative Example
[0087] Comparative Example 1
[0088] The difference from Example 1 is that the modified viscose needle felt is replaced by viscose needle felt, and the specification of the viscose needle felt is 210g / m 2 .
[0089] Comparative Example 2
[0090] The difference from Example 1 is that the copper-doped viscose fiber is replaced by copper-loaded viscose fiber, and the preparation method of the copper-loaded viscose fiber is:
[0091] The viscose fiber and nano copper were simultaneously added to excess 3-aminopropyltrihydroxysilane, the added molar amount of nano copper was consistent with the added molar amount of copper sulfate in Example 1, and then stirred for 1 hour, and finally taken out and dried to obtain copper-loaded viscose fiber.
[0092] Comparative Example 3
[0093] The difference from Example 1 is that the copper-doped viscose fiber modified by butanetetracarboxylic acid is replaced by the copper-doped viscose fiber.
[0094] Comparative Example 4
[0095] The difference from Example 1 is that the copper-doped viscose fiber is replaced by viscose fiber.
[0096] Performance testing
[0097] Detection Methods
[0098] 1. Thermal conductivity test
[0099] Three samples were taken from Examples 1-7 and Comparative Examples 1-4 respectively, and then the thermal conductivity of the samples at 1150° C. was tested by a thermal conductivity tester according to GB / T8722-2008 “Method for Determination of Medium-Temperature Thermal Conductivity of Graphite Materials” and the average value was taken.
[0100] 2. Anti-cracking performance test
[0101] The preparation operation was performed 10,000 times for Examples 1-7 and Comparative Examples 1-4, and then the surfaces of the prepared samples were observed to see whether there were cracks. The samples without cracks were considered qualified, and the qualified rate was calculated.
[0102] The test data are shown in Table 1.
[0103] Table 1 Test data table of Examples 1-7 and Comparative Examples 1-4
[0104]
[0105] Referring to Example 1 and Comparative Example 1 and in combination with Table 1, it can be seen that compared with Comparative Example 1, the thermal conductivity and the qualified rate of Example 1 are significantly improved, which shows that compared with the use of conventional viscose fiber needle felt to prepare graphite felt, the graphite felt prepared by using the modified viscose fiber needle felt of the present application will have better thermal conductivity and crack resistance.
[0106] With reference to Example 1 and Comparative Example 2 and in combination with Table 1, it can be seen that, relative to Example 1, the qualified rate of Comparative Example 2 is basically unchanged, but the thermal conductivity of Comparative Example 2 is slightly reduced. This shows that, relative to the use of copper-doped adhesive fibers, the use of copper-loaded adhesive fibers will lead to a significant deterioration in the thermal conductivity of high-purity adhesive carbon fiber composite material graphite felt.
[0107] The reason is that copper-doped viscose fiber utilizes the potential reducing groups in viscose fiber to promote the accumulation of copper in the viscose fiber cavity through an in-situ reduction reaction of copper sulfate, thereby forming aggregates or even microcrystalline structures. After the reaction, the pores of the viscose fiber shrink and copper is deposited in the viscose fiber cavity, which effectively limits the shedding of copper, thereby increasing the copper loading of the graphite felt and preparing for the subsequent 3-aminopropyltrihydroxysilane coupling and butanetetracarboxylic acid, effectively improving the thermal conductivity of high-purity viscose-based carbon fiber composite graphite felt.
[0108] The copper-loaded viscose fiber is simply prepared by physically mixing copper and viscose fiber, and then connected through 3-aminopropyltrihydroxysilane and butanetetracarboxylic acid. The adhesion of copper is relatively poor, which in turn manifests as a poor thermal conductivity.
[0109] Referring to Example 1 and Comparative Example 3 and combining with Table 1, it can be seen that compared with Example 1, the thermal conductivity and the qualified rate of Comparative Example 3 are significantly reduced, which shows that the butanetetracarboxylic acid modification operation can effectively improve the crack resistance and thermal conductivity of high-purity adhesive carbon fiber composite graphite felt.
[0110] The reason is that cracks in graphite felt occur because during the pyrolysis process of viscose fiber, viscose fiber will produce a large number of complex reactions, which will cause a large number of defect structures in the graphite felt itself, and the scattered copper will cause the defect structures to further increase, and these defect structures are one of the reasons that cause cracks in graphite felt.
[0111] After the modification of butanetetracarboxylic acid, the two adjacent carboxyl groups of butanetetracarboxylic acid are first dehydrated into anhydrides, and then the highly active cyclic anhydrides further react with the hydroxyl groups on the viscose fiber macromolecules to form esters and release a carboxyl group. The released carboxyl group can also be dehydrated with another adjacent carboxyl group to form anhydrides and connect with another hydroxyl group on the viscose fiber. At the same time, the remaining carboxyl groups can also connect with the hydroxyl groups on copper, thereby forming a multi-crosslinked network structure. While effectively increasing the copper loading of the viscose fiber, it can also effectively increase the bond content in the viscose fiber, thereby inhibiting the generation of defects during the pyrolysis process, effectively reducing the possibility of cracks in the graphite felt, and ensuring its thermal conductivity.
[0112] Referring to Example 1 and Comparative Example 4 and combining with Table 1, it can be seen that relative to Example 1, the thermal conductivity of Comparative Example 4 is significantly reduced, and the qualified rate of Comparative Example 4 is even slightly improved, which shows that the selection of copper-doped viscose fiber can effectively improve the thermal conductivity of high-purity viscose-based carbon fiber composite material graphite felt.
[0113] The reason is that the poor thermal conductivity of graphite is due to its lack of uniformity. Its thermal conductivity in the direction parallel to the plane is extremely high, but its thermal conductivity in the direction perpendicular to the plane is relatively low. Although copper is inferior to graphite in terms of maximum thermal conductivity, its uniformity is better. Therefore, after copper is doped on viscose fiber, in the pre-oxidation, carbonization and graphitization processes, the graphite felt will have better thermal conductivity overall.
[0114] Referring to Examples 1-3 and in combination with Table 1, it can be seen that, relative to Example 1, the qualified rate of Examples 2-3 is basically unchanged, but the thermal conductivity of Examples 2-3 is slightly decreased. This shows that in the preparation method of copper-doped viscose fiber, when the copper sulfate concentration, reaction temperature and reaction time are selected as the parameters of Example 1, the prepared high-purity viscose-based carbon fiber composite material graphite felt will have better thermal conductivity.
[0115] It can be seen from the parameters of Example 1 and Examples 4-5 in combination with Table 1 that, relative to Example 1, the thermal conductivity and qualified rate of Examples 4-5 are significantly reduced, which indicates that in S2, when butanetetracarboxylic acid uses the specific parameters of Example 1, the prepared high-purity viscose-based carbon fiber composite material graphite felt will have better thermal conductivity and crack resistance.
[0116] With reference to Example 1 and Examples 6-7 and in combination with Table 1, it can be seen that, relative to Example 1, the thermal conductivity of Examples 6-7 is substantially unchanged, but the qualified rates of Examples 6-7 are significantly decreased.
[0117] The reason is that, in the process of carbonization or graphitization, first performing low-temperature carbonization and then high-temperature carbonization, as well as first pre-graphitization and then graphitization, can effectively reduce the possibility of cracks in the graphite felt. The reason may be that the low-temperature carbonization process and the pre-graphitization process can effectively slow down the generation of defective structures during the pyrolysis of viscose fibers, thereby effectively reducing the possibility of cracks in the graphite felt.
[0118] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high-purity viscose-based carbon fiber composite material graphite felt, characterized in that: The high-purity viscose-based carbon fiber composite material graphite felt is prepared by pre-oxidation, carbonization and graphitization of modified viscose fiber needle-punched felt; The modified viscose fiber needle-punched felt is prepared by a needle-punching process of copper-doped viscose fiber modified with butanetetracarboxylic acid, and the copper of the copper-doped viscose fiber contains hydroxyl groups; The preparation method of the copper-doped viscose fiber is as follows: soaking the viscose fiber in a penetrant JFC solution, treating it at a temperature of 30-40° C. for 10-30 minutes, then washing and drying it, then putting it into a copper sulfate solution, shaking it for reaction, then washing it, soaking it again in 3-aminopropyltrihydroxysilane, and finally drying it to obtain the copper-doped viscose fiber; The mass ratio of the viscose fiber to the penetrant JFC solution is 1:(100-120), and the content of JFC in the penetrant JFC solution is 1-3%; The preparation method of the butanetetracarboxylic acid modified copper-doped viscose fiber comprises the following steps: S1. First, soak the copper-doped viscose fiber in a sodium sulfite aqueous solution at a soaking temperature of 70-80° C. for 1-2 h, and then wash with water to obtain the pretreated copper-doped viscose fiber; S2, performing a three-immersion and three-rolling treatment on the pretreated copper-doped viscose fiber, wherein the immersion solution contains butane tetracarboxylic acid and sodium hypophosphite, and then drying at 40-50° C. to a constant weight to obtain butane tetracarboxylic acid-copper-doped viscose fiber; S3, transferring the butanetetracarboxylic acid-copper-doped viscose fiber to a temperature of 150-210° C. for crosslinking for 3-6 minutes, and finally washing and drying for equilibrium to obtain butanetetracarboxylic acid-modified copper-doped viscose fiber.
2. The high-purity viscose-based carbon fiber composite material graphite felt according to claim 1, characterized in that: The concentration of the copper sulfate solution is 3.5-4.5 mmol / L, the oscillation reaction temperature is 85-95° C., and the oscillation reaction time is 90-150 min.
3. The high-purity viscose-based carbon fiber composite material graphite felt according to claim 1, characterized in that: In S1, the concentration of the sodium sulfite aqueous solution is 20-30 g / L, and the mass ratio of the copper-doped viscose fiber to the sodium sulfite aqueous solution is 1:(100-120).
4. The high-purity viscose-based carbon fiber composite material graphite felt according to claim 1, characterized in that: In S2, the mass ratio of butane tetracarboxylic acid to sodium hypophosphite is (1-2):1, the content of butane tetracarboxylic acid in the soaking solution is 5-10%, and the mass ratio of the pretreated copper-doped viscose fiber to the soaking solution is 1:(40-50).