Natural collagen-polyphosphate composite sponge and application thereof

Through the cross-linking of natural collagen and oligopolymerized polyphosphate in calcium chloride solution and nanosilver loading, a composite sponge was formed, which solved the problems of poor mechanical properties and insufficient antibacterial properties of a single dressing of natural collagen, and realized the composite sponge The high mechanical properties and long-lasting antibacterial effects significantly improve hemostatic performance.

CN118976144APending Publication Date: 2024-11-19ZHEJIANG NAJI BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411124951.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing single dressings of natural collagen have poor mechanical properties and lack antibacterial properties, which is difficult to meet clinical needs. The application of nanosilver in the system can easily lead to fluctuations in antibacterial properties and natural collagen aggregation. The hemostatic performance of polyphosphate depends on high polymerization degree. Moreover, the solubility is low, making it difficult to form a stable structure with other polymer materials.

Method used

Using the preparation method of natural collagen-polyphosphate composite sponge, the nano-laden nano-silver is formed by cross-linking natural collagen and oligopolymerized polyphosphate in calcium chloride solution, and adding nano-silver to some examples. Natural collagen-polyphosphate composite sponge improves mechanical properties and antibacterial effects.

Benefits of technology

It significantly improves the mechanical properties of natural collagen and the coagulation properties of phosphate with low polymerization degree, avoids the failure of nano-silver agglomeration, and achieves long-lasting antibacterial effects and excellent hemostatic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976144A_ABST
    Figure CN118976144A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of biological materials, and discloses a natural collagen-polyphosphate composite sponge and application thereof. The inventor finds that by adding polyphosphate into a natural collagen solution and immersing the natural collagen solution into a calcium chloride solution for crosslinking, the mechanical property of a natural collagen material can be remarkably improved, and the prepared natural collagen-polyphosphate composite sponge has good mechanical property; the natural collagen-polyphosphate composition also unexpectedly improves the coagulation performance of the phosphate with low polymerization degree, and improves the hemostatic performance of the composite sponge. The nano-silver is loaded on the natural collagen through in-situ reaction, so that the agglomeration failure of the nano-silver is avoided. And the generated nano-silver is protected by the composite sponge, and the antibacterial effect is more durable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of biomaterials, and in particular relates to a natural collagen-polyphosphate composite sponge and an application thereof. Background Art

[0002] Wound healing and tissue repair are one of the key issues facing military and civilian medicine, and have a very important impact on human life support and physical health. Hemostatic sponges are widely used in wound healing and tissue repair due to their porous structure, high mechanical strength and good wound repair performance, and have become an important branch of wound dressing materials. In recent years, natural polymers, artificial synthetic polymers and other materials have been widely used in the preparation of hemostatic materials. Among them, bio-based polymer materials extracted from animals and plants or synthesized from bio-based monomers have attracted great attention due to their good biocompatibility, biodegradability and bioabsorbability, and are widely made into hemostatic materials and wound dressings with functions such as hemostasis, protection and promotion of wound healing.

[0003] Natural collagen is one of the most abundant proteins in multicellular organisms and is widely found in animal skin, bones and other tissues. The unique triple helix structure of natural collagen gives it excellent biodegradability, cell adaptability, biocompatibility, low antigenicity, and the ability to promote cell proliferation and accelerate platelet aggregation. It has become the main component of many wound repair materials and has been developed into wound dressings in various forms such as hemostatic sponges, gels, and films. Although natural collagen has many advantages, single-component natural collagen-based dressings often have poor mechanical properties and almost no antibacterial properties, making it difficult to fully meet the needs of clinical practice. In order to improve the mechanical properties of single natural collagen, grafting modification, doping and blending are often used to improve its performance. Grafting modification often requires harsh reaction conditions (high temperature, strong acid and alkali, etc.), which can easily lead to the loss or destruction of the triple helix structure of natural collagen, thereby reducing its biological activity; due to the differences in physical properties of different compounds, if the doping material or doping conditions are not properly selected, it is difficult to form a uniform system, which can easily lead to the aggregation of natural collagen and weaken its biological activity.

[0004] Nanosilver particles have strong inhibitory and killing effects on dozens of pathogenic microorganisms such as Staphylococcus aureus and Escherichia coli, and do not produce drug resistance. They are often used to improve the antibacterial properties of materials. However, when nanosilver particles are introduced into other systems, changes in pH, ionic strength, etc. can easily lead to nanosilver aggregation, which greatly affects its antibacterial properties. In addition, the introduction of nanosilver may also cause natural collagen to aggregate, thereby affecting the hemostatic properties of natural collagen.

[0005] Polyphosphate is a linear phosphate polymer composed of high-energy phosphate monomers, which is widely present in animals, plants and microorganisms including the human body. Polyphosphate has the effect of activating the endogenous coagulation pathway, accelerating thrombin generation, and enhancing the structural strength and stability of fibrin, and can be used for wound repair and wound healing medical dressing materials. However, the hemostatic performance of polyphosphate has a strong polymerization degree dependence, and polyphosphates with high polymerization degree have excellent coagulation performance, while polyphosphates with low polymerization degree (average polymerization degree 50 and below) have poor coagulation performance and weak antibacterial properties. However, the solubility of polyphosphates with high polymerization degree is low, the viscosity is large, it is difficult to prepare molding, and it is also difficult to form a stable and uniform structure with other polymer materials, which also limits the scope of application of high polymerization degree polyphosphates. Summary of the invention

[0006] The purpose of the present invention is to overcome at least one disadvantage of the prior art and provide a natural collagen-polyphosphate composite sponge and its application.

[0007] The technical solution adopted by the present invention is:

[0008] A natural collagen-polyphosphate composite sponge, the preparation method of which comprises the following steps:

[0009] S1) dissolving natural collagen to obtain a natural collagen solution;

[0010] S2) dissolving polyphosphate in water to obtain a polyphosphate solution;

[0011] S3) mixing the natural collagen solution and the polyphosphate solution, and transferring the mixture into a mold containing a calcium chloride solution for cross-linking;

[0012] S4) After the cross-linking is completed, the mixture is washed and freeze-dried to obtain a natural collagen-polyphosphate composite sponge.

[0013] In some examples of natural collagen-polyphosphate composite sponges, the preparation method thereof comprises the following steps:

[0014] S1-1) dissolving natural collagen to obtain a natural collagen solution;

[0015] S1-1) adding silver nitrate solution to the natural collagen solution, mixing well, adding reducing agent, mixing well, and reducing to obtain a natural collagen mixed solution loaded with nanosilver;

[0016] S1-1) dialysis purifies the mixed solution of natural collagen loaded with nano-silver to obtain a natural collagen solution loaded with nano-silver;

[0017] S2) dissolving polyphosphate in water to obtain a polyphosphate solution;

[0018] S3) mixing the natural collagen solution loaded with nanosilver and the polyphosphate solution, and transferring the mixture to a mold filled with a calcium chloride solution for cross-linking;

[0019] S4) After the cross-linking is completed, the mixture is washed and freeze-dried to obtain a natural collagen-polyphosphate composite sponge loaded with nanosilver.

[0020] In some examples of the natural collagen-polyphosphate composite sponge, the concentration of natural collagen is 1-5 mg / mL.

[0021] In some examples of natural collagen-polyphosphate composite sponges, the concentration of polyphosphate is 5-20 mg / mL.

[0022] In some examples of natural collagen-polyphosphate composite sponges, the concentration of natural collagen is 1-5 mg / mL, and the concentration of polyphosphate is 5-20 mg / mL.

[0023] In some examples of natural collagen-polyphosphate composite sponges, the degree of polymerization of the polyphosphate is 20-10000, preferably 20-50.

[0024] In some examples of natural collagen-polyphosphate composite sponges, the reducing agent is at least one of sodium borohydride and ascorbic acid.

[0025] In some examples of natural collagen-polyphosphate composite sponges, the concentration of silver nitrate is 2-10 mmol / L.

[0026] In some examples of natural collagen-polyphosphate composite sponges, the reducing agent is at least one of sodium borohydride and ascorbic acid, and the concentration of the silver nitrate is 2-10 mmol / L.

[0027] In some examples of natural collagen-polyphosphate composite sponges, the mass ratio of natural collagen to polyphosphate is (10-20):1.

[0028] The above features can be combined arbitrarily as long as they do not conflict with each other.

[0029] The second aspect of the present invention provides:

[0030] The first aspect of the present invention is the use of the natural collagen-polyphosphate composite sponge in the preparation of wound repair materials.

[0031] The beneficial effects of the present invention are:

[0032] The natural collagen-polyphosphate composite sponges in some examples of the present invention significantly improve the mechanical properties of the natural collagen material by adding polyphosphate and immersing in a calcium chloride solution for cross-linking, and the prepared natural collagen-polyphosphate composite sponges have good mechanical properties; the natural collagen-polyphosphate composite also unexpectedly improves the coagulation properties of low-polymerization degree phosphates and improves the hemostatic properties of the composite sponge.

[0033] The natural collagen-polyphosphate composite sponge of some embodiments of the present invention prevents the failure of nanosilver aggregation by loading nanosilver. The nanosilver is also protected by the composite sponge, and the antibacterial effect is more lasting. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a scanning electron microscope image of the composite sponge obtained in Example 1.

[0035] Figure 2 The following is a comparison of the antibacterial rates of the composite sponge obtained in Example 1 and the corresponding natural collagen (Col), polyphosphate (Poly-P) and natural protein / polyphosphate composite material (Col / Poly-P) against Staphylococcus aureus. Natural collagen has almost no antibacterial effect, polyphosphate has a certain antibacterial effect, and the antibacterial rate against Staphylococcus aureus is 85.2%, the antibacterial rate of the natural protein / polyphosphate composite material is only 64.8%, and the natural collagen / polyphosphate composite material (Ag-Col / Poly-P) loaded with nanosilver has a good antibacterial effect, and the antibacterial rate can reach 98.3%.

[0036] Figure 3 The figure is a comparison of the tensile strength of the composite sponge obtained in Example 1 and the corresponding natural collagen and natural protein / polyphosphate composite materials. The introduction of polyphosphate significantly improves the tensile strength of natural collagen and the mechanical properties of the material, and the intervention of nanosilver has little effect on the mechanical properties of the composite material.

[0037] Figure 4 The figure is a comparison of the coagulation index of the composite sponge and polyphosphate obtained in Example 1, and the composite material of natural protein and polyphosphate. The anticoagulated blood was activated with calcium chloride, and then the sample was added and incubated at 37°C. The supernatant was taken and the absorbance at 545nm was tested. The group without sample was the control group. The ratio of the sample group to the control group was the coagulation index. The smaller the coagulation index, the better the hemostatic performance. The synergistic effect of natural collagen and polyphosphate significantly reduced the coagulation index of the material, showing an excellent hemostatic effect. DETAILED DESCRIPTION

[0038] A natural collagen-polyphosphate composite sponge, the preparation method of which comprises the following steps:

[0039] S1) dissolving natural collagen to obtain a natural collagen solution;

[0040] S2) dissolving polyphosphate in water to obtain a polyphosphate solution;

[0041] S3) mixing the natural collagen solution and the polyphosphate solution, and transferring the mixture into a mold containing a calcium chloride solution for cross-linking;

[0042] S4) After the cross-linking is completed, washing and freeze-drying are performed to obtain a natural collagen-polyphosphate composite sponge.

[0043] In some examples of natural collagen-polyphosphate composite sponges, the preparation method thereof comprises the following steps:

[0044] S1-1) dissolving natural collagen to obtain a natural collagen solution;

[0045] S1-1) adding silver nitrate solution to the natural collagen solution, mixing well, adding reducing agent, mixing well, and reducing to obtain a natural collagen mixed solution loaded with nanosilver;

[0046] S1-1) dialysis purifies the mixed solution of natural collagen loaded with nano-silver to obtain a natural collagen solution loaded with nano-silver;

[0047] S2) dissolving polyphosphate in water to obtain a polyphosphate solution;

[0048] S3) mixing the natural collagen solution loaded with nanosilver and the polyphosphate solution, and transferring the mixture to a mold filled with a calcium chloride solution for cross-linking;

[0049] S4) After the cross-linking is completed, the mixture is washed and freeze-dried to obtain a natural collagen-polyphosphate composite sponge loaded with nanosilver.

[0050] In order to avoid denaturation and inactivation of natural collagen, it is preferably prepared at an environment not higher than 15°C.

[0051] In some examples of natural collagen-polyphosphate composite sponges, the concentration of natural collagen is 1-5 mg / mL, which can ensure sufficient concentration.

[0052] Natural collagen is natural type I collagen with a complete triple helix molecular structure. There is no special requirement for its source. It can be extracted, separated and purified from the skin and Achilles tendon tissue of mammals, fish and amphibians.

[0053] In some examples of natural collagen-polyphosphate composite sponges, the concentration of polyphosphate is 5-20 mg / mL.

[0054] In some examples of natural collagen-polyphosphate composite sponges, the concentration of natural collagen is 1-5 mg / mL, and the concentration of polyphosphate is 5-20 mg / mL.

[0055] In some examples of natural collagen-polyphosphate composite sponges, the degree of polymerization of the polyphosphate is 20-10000, preferably 20-50. The use of low-degree-of-polymerization polyphosphate with a degree of polymerization of 20-50 has better solubility and can be better composited with natural collagen.

[0056] In some examples of natural collagen-polyphosphate composite sponges, the reducing agent is at least one of sodium borohydride and ascorbic acid.

[0057] In some examples of natural collagen-polyphosphate composite sponges, the concentration of silver nitrate is 2-10 mmol / L.

[0058] In some examples of natural collagen-polyphosphate composite sponges, the reducing agent is at least one of sodium borohydride and ascorbic acid, and the concentration of the silver nitrate is 2-10 mmol / L.

[0059] In some examples of natural collagen-polyphosphate composite sponges, the mass ratio of natural collagen to polyphosphate is (10-20):1.

[0060] The cross-linking time can be adjusted accordingly according to the concentration of natural collagen, polyphosphate, and calcium chloride, so as to achieve the desired degree of cross-linking. The specific cross-linking time can be further determined by testing the cross-linking of the product. In some examples of natural collagen-polyphosphate composite sponges, the cross-linking time is 5 min-8 h.

[0061] In order to obtain a better cross-linking speed, in some examples of natural collagen-polyphosphate composite sponges, the concentration of the calcium chloride solution is 1-5 wt %.

[0062] The purpose of dialysis purification is to remove unreacted small molecules. In some examples of natural collagen-polyphosphate composite sponges, the molecular weight cutoff for dialysis purification is 8000-15000 Daltons. To ensure sufficient removal of small molecules, it is preferred to dialyze for 24-72 hours, and replace the dialysate every 5-6 hours.

[0063] The above features can be combined arbitrarily as long as they do not conflict with each other.

[0064] The technical solution of the present invention is further explained below in conjunction with examples.

[0065] Example 1

[0066] Weigh an appropriate amount of natural bovine Achilles tendon collagen sample, dissolve it with 0.1mol / L acetic acid solution to form 10mL of bovine Achilles tendon collagen solution with a concentration of 1mg / mL, add 1mL of 4mmol silver nitrate solution and stir for 2h, slowly add 0.5mL of 0.2mol / L sodium borohydride solution, stir and react for 18 hours, then put it into a dialysis bag with a molecular weight cutoff of 12000 Daltons, use deionized water as the dialysate, replace the dialysate every 6h, and dialyze for 48 hours to obtain a natural collagen solution loaded with nanosilver.

[0067] Another sodium polyphosphate sample with an average degree of polymerization of 25 was weighed, prepared into 1 mL of a solution with a concentration of 10 mg / mL with deionized water, and then mixed with the natural collagen solution loaded with nanosilver and transferred to a mold filled with a 2% wt calcium chloride solution for cross-linking for 1 hour, and then washed with deionized water for 3 times, pre-frozen at -20°C, and after the sample was completely frozen, transferred to a freeze drying oven, and continued to freeze-dry at -55°C for 48 hours to obtain a natural collagen / polyphosphate composite sponge loaded with nanosilver.

[0068] Example 2

[0069] Weigh an appropriate amount of natural pig skin collagen sample, dissolve it with 0.2 mol / L acetic acid solution to form 15 mL of bovine Achilles tendon collagen solution with a concentration of 2 mg / mL, add 1 mL of 3 mmol silver nitrate solution and stir for 1 hour, slowly add 0.8 mL of 0.1 mol / L sodium borohydride solution, stir and react for 15 hours, then put it into a dialysis bag with a molecular weight cutoff of 12000 Daltons, use deionized water as the dialysate, replace the dialysate every 6 hours, and dialyze for 48 hours to obtain a natural collagen solution loaded with nanosilver.

[0070] Weigh another sodium polyphosphate sample with an average degree of polymerization of 50, prepare it into 1.5 mL of a solution with a concentration of 5 mg / mL with deionized water, mix it with the natural collagen solution loaded with nanosilver, and transfer it to a mold filled with 2% wt calcium chloride solution for cross-linking for 0.5 h, then wash it with deionized water for 3 times, pre-freeze it at -20°C, transfer it to a freeze drying oven after the sample is completely frozen, and continue freeze-drying at -55°C for 48 h to obtain a natural collagen / polyphosphate composite sponge loaded with nanosilver.

[0071] Example 3

[0072] Weigh an appropriate amount of natural bullfrog skin protein sample, dissolve it with 0.5 mol / L acetic acid solution to form 10 mL of bovine Achilles tendon collagen solution with a concentration of 4 mg / mL, add 1 mL of 5 mmol silver nitrate solution and stir for 2 h, slowly add 1 mL of 0.2 mol / L sodium borohydride solution, stir and react for 24 hours, then put it into a dialysis bag with a molecular weight cutoff of 12000 Daltons, use deionized water as the dialysate, replace the dialysate every 6 hours, and dialyze for 48 hours to obtain a natural collagen solution loaded with nanosilver.

[0073] Another sodium polyphosphate sample with an average degree of polymerization of 25 was weighed, prepared into 1 mL of a solution with a concentration of 10 mg / mL with deionized water, and then mixed with the natural collagen solution loaded with nanosilver and transferred to a mold filled with a 3%wt calcium chloride solution for cross-linking for 2 hours. The mold was then washed with deionized water for 3 times and pre-frozen at -20°C. After the sample was completely frozen, it was transferred to a freeze drying oven and freeze-dried at -55°C for 48 hours to obtain a natural collagen / polyphosphate composite sponge loaded with nanosilver.

[0074] Example 4

[0075] Weigh an appropriate amount of natural bovine Achilles tendon collagen sample, dissolve it in 0.1 mol / L acetic acid solution to obtain 10 mL of 1 mg / mL bovine Achilles tendon collagen solution, use deionized water as the dialysate, replace the dialysate every 6 hours, and dialyze for 48 hours to obtain a natural collagen solution;

[0076] Weigh another sodium polyphosphate sample with an average degree of polymerization of 25, prepare it into 1 mL of a solution with a concentration of 10 mg / mL with deionized water, mix it with the natural collagen solution, and transfer it to a mold filled with 2% wt calcium chloride solution for cross-linking for 1 hour. Then wash it with deionized water for 3 times, pre-freeze it at -20°C, transfer it to a freeze drying oven after the sample is completely frozen, and continue freeze-drying at -55°C for 48 hours to obtain a natural collagen / polyphosphate composite sponge.

[0077] Comparative Example 1

[0078] Weigh an appropriate amount of natural bovine Achilles tendon collagen sample, dissolve it with 0.1mol / L acetic acid solution to form 10mL of 1mg / mL bovine Achilles tendon collagen solution, add 1mL of nanosilver solution (obtained by reduction reaction of 1mL 4mmol silver nitrate solution and 0.5mL 0.2mol / L sodium borohydride solution), put it into a dialysis bag with a molecular weight cutoff of 12000 Daltons, use deionized water as the dialysate, replace the dialysate every 6h, and dialyze for 48 hours to obtain a natural collagen solution loaded with nanosilver.

[0079] Another sodium polyphosphate sample with an average degree of polymerization of 25 was weighed, prepared into 1 mL of a solution with a concentration of 10 mg / mL with deionized water, and then mixed with the natural collagen solution loaded with nanosilver and transferred to a mold filled with a 2% wt calcium chloride solution for cross-linking for 1 hour, and then washed with deionized water for 3 times, pre-frozen at -20°C, and after the sample was completely frozen, transferred to a freeze drying oven, and continued to freeze-dry at -55°C for 48 hours to obtain a natural collagen / polyphosphate composite sponge loaded with nanosilver.

[0080] The antibacterial experiment showed that the antibacterial rate of the obtained sample against Staphylococcus aureus was only 72.6%, which was significantly lower than the solution (98.3%) proposed by the present invention.

[0081] Performance Test:

[0082] Figure 1 The scanning electron microscope image of the composite sponge obtained in Example 1. The prepared composite sponge was sliced ​​into thin slices to obtain a complete cross section, and the surface was sprayed with gold, and the morphology was observed using a scanning electron microscope. The prepared composite sponge exhibited a three-dimensional porous structure, which was helpful for absorbing blood and accelerating the adhesion and aggregation of red blood cells and platelets.

[0083] Figure 2 The following is a comparison of the antibacterial rates of the composite sponge obtained in Example 1 and the corresponding natural collagen (Col), polyphosphate (Poly-P) and natural protein / polyphosphate composite material (Col / Poly-P) against Staphylococcus aureus. Natural collagen has almost no antibacterial effect, polyphosphate has a certain antibacterial effect, and the antibacterial rate against Staphylococcus aureus is 85.2%, the antibacterial rate of the natural protein / polyphosphate composite material is only 64.8%, and the natural collagen / polyphosphate composite material (Ag-Col / Poly-P) loaded with nanosilver has a good antibacterial effect, and the antibacterial rate can reach 98.3%.

[0084] Figure 3 The figure is a comparison of the tensile strength of the composite sponge obtained in Example 1 and the corresponding natural collagen and natural protein / polyphosphate composite materials. The introduction of polyphosphate significantly improves the tensile strength of natural collagen and the mechanical properties of the material, and the intervention of nanosilver has little effect on the mechanical properties of the composite material.

[0085] Figure 4The figure is a comparison of the coagulation index of the composite sponge and polyphosphate obtained in Example 1, and the composite material of natural protein and polyphosphate. The anticoagulated blood was activated with calcium chloride, and then the sample was added and incubated at 37°C. The supernatant was taken and the absorbance at 545nm was tested. The group without sample was the control group. The ratio of the sample group to the control group was the coagulation index. The smaller the coagulation index, the better the hemostatic performance. The synergistic effect of natural collagen and polyphosphate significantly reduced the coagulation index of the material, showing an excellent hemostatic effect.

[0086] The above is a further detailed description of the present invention, which should not be regarded as a limitation on the specific implementation of the present invention. For ordinary technicians in the technical field to which the present invention belongs, simple deduction or replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A natural collagen-polyphosphate composite sponge, It is characterized in that The preparation method thereof comprises the following steps: S1) dissolving natural collagen to obtain a natural collagen solution; S2) dissolving polyphosphate in water to obtain a polyphosphate solution; S3) mixing the natural collagen solution and the polyphosphate solution, and transferring the mixture into a mold containing a calcium chloride solution for cross-linking; S4) After the cross-linking is completed, the mixture is washed and freeze-dried to obtain a natural collagen-polyphosphate composite sponge.

2. The natural collagen-polyphosphate composite sponge according to claim 1, It is characterized in that The preparation method thereof comprises the following steps: S1-1) dissolving natural collagen to obtain a natural collagen solution; S1-1) adding silver nitrate solution to the natural collagen solution, mixing well, adding reducing agent, mixing well, and reducing to obtain a natural collagen mixed solution loaded with nanosilver; S1-1) dialysis purifies the mixed solution of natural collagen loaded with nano-silver to obtain a natural collagen solution loaded with nano-silver; S2) dissolving polyphosphate in water to obtain a polyphosphate solution; S3) mixing the natural collagen solution loaded with nanosilver and the polyphosphate solution, and transferring the mixture to a mold filled with a calcium chloride solution for cross-linking; S4) After the cross-linking is completed, the mixture is washed and freeze-dried to obtain a natural collagen-polyphosphate composite sponge loaded with nanosilver.

3. The natural collagen-polyphosphate composite sponge according to claim 1 or 2, It is characterized in that The concentration of native collagen is 1-5 mg / mL; and / or the concentration of polyphosphate is 5-20 mg / mL.

4. The natural collagen-polyphosphate composite sponge according to claim 1 or 2, It is characterized in that The degree of polymerization of polyphosphate is 20-10000.

5. The natural collagen-polyphosphate composite sponge according to claim 1 or 2, It is characterized in that During the preparation process, the temperature was controlled not to exceed 15°C.

6. The natural collagen-polyphosphate composite sponge according to claim 1 or 2, It is characterized in that The concentration of the calcium chloride solution is 1-5 wt%.

7. The natural collagen-polyphosphate composite sponge according to claim 4, It is characterized in that The degree of polymerization of polyphosphate is 20-50.

8. The natural collagen-polyphosphate composite sponge according to claim 2, It is characterized in that The reducing agent is sodium borohydride and / or ascorbic acid; and / or The concentration of the silver nitrate is 2-10 mmol / L.

9. The natural collagen-polyphosphate composite sponge according to claim 1 or 2, It is characterized in that The mass ratio of natural collagen to polyphosphate is (10-20):

1.

10. Use of the natural collagen-polyphosphate composite sponge according to any one of claims 1 to 9 in the preparation of wound repair materials.