Ze-MOFs material for cobalt ion separation and preparation method thereof
By preparing Ze-MOFs materials composed of zeolites and organic ligands, the problem of insufficient cobalt ion removal ability in water is solved, efficient and environmentally friendly cobalt ion adsorption and separation is achieved, and the use of waste batteries is promoted. Recycling and resource recycling.
Patent Information
- Application Number
- CN202411086783.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing adsorbents have insufficient adsorption capacity, poor selectivity, slow adsorption speed and lack environmental friendliness when removing cobalt ions in water, making it difficult to effectively deal with cobalt ions in waste ternary lithium batteries.
Ze-MOFs materials composed of zeolite, terephthalic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid were prepared by artificial activation, crushing and hydrothermal reaction to form Ze-MIL- Materials of 53(Al), Ze-MIL-53(Al)-NH2, Ze-MIL-53(Al)-(OH)2 and other types are used for efficient adsorption and separation of cobalt ions.
It has achieved efficient adsorption of cobalt ions, with an adsorption capacity of up to 92.67mg/g. It has low price and environmentally friendly characteristics, and is suitable for recycling and resource recycling of waste ternary lithium batteries.
Smart Images

Figure CN118976474A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery processing, and in particular to a Ze-MOFs material for cobalt ion separation and a preparation method thereof. Background Art
[0002] With the rapid development of electric vehicles and renewable energy, the treatment and recycling of spent ternary lithium batteries, a common type of lithium-ion batteries, has attracted widespread attention; these batteries contain important metal elements such as cobalt, especially cobalt, which not only has a wide range of applications in industry, but also has problems of environmental toxicity and resource waste.
[0003] Without effective treatment and recycling, the cobalt ions in waste ternary lithium batteries may have negative effects on the environment and human health. Therefore, it is crucial to develop methods to efficiently remove cobalt ions from waste batteries, which can not only achieve the recycling of valuable metal resources, but also help reduce environmental pollution and resource waste. This research not only promotes the recycling of waste batteries, but also provides support for the establishment of a circular economy system and a sustainable development model. Traditional separation methods such as solvent extraction, ion exchange and membrane separation have problems such as complex operation, high cost and environmental pollution.
[0004] With the development of technology, adsorption materials have attracted much attention in recent years as a green and efficient separation technology. By synthesizing adsorption materials with specific structures and functions, such as MOFs and Ze-MOFs, efficient adsorption and separation of cobalt ions can be achieved. It has the advantages of large adsorption capacity and strong selectivity, and has therefore become one of the current research hotspots.
[0005] Although a variety of existing adsorbents have been used to remove cobalt ions from water, they still have problems such as insufficient adsorption capacity, poor selectivity, slow adsorption rate and lack of environmental friendliness. Summary of the invention
[0006] The purpose of the present invention is to provide a Ze-MOFs material for cobalt ion separation and a preparation method thereof, aiming to solve the technical problems that various adsorbents in the prior art are used to remove cobalt ions in water bodies, but have insufficient adsorption capacity, poor selectivity, slow adsorption rate and lack of environmental friendliness.
[0007] To achieve the above object, the present invention adopts a Ze-MOFs material for cobalt ion separation, which includes zeolite Zeolite, terephthalic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid.
[0008] The present invention also provides a method for preparing a Ze-MOFs material for cobalt ion separation, which is used to prepare the Ze-MOFs material for cobalt ion separation as described above, characterized in that:
[0009] The steps include:
[0010] Step 1: Activation of artificial zeolite: Place the zeolite in a crucible, place it in a muffle furnace for activation, and then cool it to room temperature;
[0011] Step 2: crushing the artificial zeolite: grinding the cooled zeolite in a ball mill, and collecting the powder after grinding;
[0012] Step 3: First, disperse the powdered zeolite and organic ligand into deionized water, stir them thoroughly at room temperature to evenly disperse the zeolite and organic ligand, then add acetic acid, transfer them into a hydrothermal reactor with polytetrafluoroethylene for reaction, recover the material after the reaction is completed, wash the material with deionized water 2-3 times, and vacuum dry it to obtain Ze-MOFs material for cobalt ion separation.
[0013] Wherein, in step 1, the zeolite is placed in a crucible and placed in a muffle furnace for activation at a temperature of 800° C. and an activation time of 10 hours.
[0014] Wherein, in step 2, the grinding rate is 320 rpm and the grinding time is 5 h.
[0015] Wherein, in step three, the reaction temperature in the hydrothermal reactor is 120° C., and the reaction time is 24 hours.
[0016] Among them, in step three, after the reaction in the hydrothermal reactor is completed, the material is recovered by centrifugal separation.
[0017] Wherein, the organic ligand includes terephthalic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid.
[0018] Wherein, the Ze-MOFs material is one of Ze-MIL-53(Al), Ze-MIL-53(Al)-NH2, and Ze-MIL-53(Al)-(OH)2.
[0019] The invention discloses a Ze-MOFs material for separating cobalt ions and a preparation method thereof. First, zeolite is placed in a crucible, placed in a muffle furnace for activation, and then cooled to room temperature. Then, the zeolite is ground by a ball mill to obtain a powdered zeolite Zeolite with a smaller particle size. The zeolite Zeolite and an organic ligand (terephthalic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid) are placed in a reactor for hydrothermal reaction to obtain zeolite-based metal-organic framework materials Ze-MOFs (Ze-MIL-53(Al), Ze-MIL-53(Al)-NH2, Ze-MIL-53(Al)-(OH)2). Finally, the Ze-MOFs material for removing cobalt ions from a waste ternary lithium battery leachate is obtained. When the Ze-MOFs material for removing cobalt ions from a leachate is used to remove cobalt ions in wastewater, the Co-containing 2+ The pH value of the solution is adjusted to 5.0-9.0, and the de-Ze-MOFs adsorbent is added to the Co-containing 2+ Adsorption treatment is performed to adsorb Co 2+ The time is not less than 12 hours. The prepared Ze-MOFs material has the characteristics of low price and high adsorption capacity, and can be effectively used to treat cobalt ions in the leachate of waste ternary batteries, thereby promoting the recycling and resource recovery of waste batteries, and solving the technical problems of various adsorbents in the prior art being used to remove cobalt ions in water bodies, but having insufficient adsorption capacity, poor selectivity, slow adsorption speed and lack of environmental friendliness. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 It is the XRD diagram of the Ze-MOFs material with cobalt ions removed according to the present invention.
[0022] Figure 2 It is the FT-IR graph of the Ze-MOFs material with cobalt ions removed according to the present invention.
[0023] Figure 3 It is a SEM picture of the Ze-MOFs material with cobalt ions removed according to the present invention.
[0024] Figure 4 It is the EDS and Mapping diagram of the Ze-MOFs material for removing cobalt ions of the present invention and its raw materials.
[0025] Figure 5 This is a graph showing the effect of different pH values on the adsorption of cobalt ions by the Ze-MOFs material for removing cobalt ions of the present invention.
[0026] Figure 6 This is a graph showing the effect of different temperatures on the adsorption of cobalt ions by the Ze-MOFs material for removing cobalt ions of the present invention.
[0027] Figure 7 This is a graph showing the effect of different time periods on the adsorption of cobalt ions by the Ze-MOFs material for removing cobalt ions according to the present invention.
[0028] Figure 8 This is a graph showing the effect of different cobalt ion concentrations on the adsorption of cobalt ions by the Ze-MOFs material for removing cobalt ions of the present invention. DETAILED DESCRIPTION
[0029] Embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0030] The invention provides a Ze-MOFs material for separating cobalt ions, comprising zeolite Zeolite, terephthalic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid.
[0031] See also Figure 1-Figure 4 , Figure 1 is an XRD diagram of the Ze-MOFs material with cobalt ions removed according to the present invention; Figure 2 is the FT-IR graph of the Ze-MOFs material with cobalt ions removed according to the present invention; Figure 3 is a SEM image of the Ze-MOFs material with cobalt ions removed according to the present invention; Figure 4 It is the EDS and Mapping diagram of the Ze-MOFs material for removing cobalt ions and its raw materials of the present invention.
[0032] The present invention also provides a method for preparing a Ze-MOFs material for cobalt ion separation, which is used to prepare the Ze-MOFs material for cobalt ion separation as described above, characterized in that:
[0033] The steps include:
[0034] Step 1: Activation of artificial zeolite: Place the zeolite in a crucible, place it in a muffle furnace for activation, and then cool it to room temperature;
[0035] Step 2: crushing the artificial zeolite: grinding the cooled zeolite in a ball mill, and collecting the powder after grinding;
[0036] Step 3: First, disperse the powdered zeolite and organic ligand into deionized water, stir them thoroughly at room temperature to evenly disperse the zeolite and organic ligand, then add acetic acid, transfer them into a hydrothermal reactor with polytetrafluoroethylene for reaction, recover the material after the reaction is completed, wash the material with deionized water 2-3 times, and vacuum dry it to obtain Ze-MOFs material for cobalt ion separation.
[0037] Embodiment 1:
[0038] In step three, the amount of the powdered zeolite is 0.4 g, the amount of terephthalic acid is 0.8 g, the amount of acetic acid is 5 mL, and the amount of deionized water is 500 mL; the Ze-MOFs material for cobalt ion separation prepared in this embodiment is Ze-MIL-53 (Al).
[0039] Embodiment 2:
[0040] In step three, the amount of the powdered zeolite is 0.4 g, the amount of 2-aminoterephthalic acid is 1.0 g, the amount of acetic acid is 5 mL, and the amount of deionized water is 500 mL; the Ze-MOFs material for cobalt ion separation prepared in this embodiment is Ze-MIL-53(Al)-NH2.
[0041] Embodiment 3:
[0042] In step three, the amount of the powdered zeolite is 0.4 g, the amount of 2,5-dihydroxyterephthalic acid is 0.58 g, the amount of acetic acid is 5 mL, and the amount of deionized water is 500 mL; the Ze-MOFs material for cobalt ion separation prepared in this embodiment is Ze-MIL-53(Al)-(OH)2.
[0043] The Ze-MOFs material for separating cobalt ions of the present invention and the preparation method thereof are as follows: firstly, zeolite is placed in a crucible, placed in a muffle furnace for activation, and then cooled to room temperature, and then ground by a ball mill to obtain a powdered zeolite Zeolite with a smaller particle size; the zeolite Zeolite is evenly dispersed with organic ligands (terephthalic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid) and then placed in a reactor for hydrothermal reaction to obtain zeolite-based metal-organic framework materials Ze-MOFs (Ze-MIL-53(Al), Ze-MIL-53(Al)-NH2, Ze-MIL-53(Al)-(OH)2); finally, the Ze-MOFs material for removing cobalt ions from the leachate of waste ternary lithium batteries is obtained; when the Ze-MOFs material for removing cobalt ions from the leachate is used to remove cobalt ions in wastewater, the Co-containing 2+The pH value of the solution is adjusted to 5.0-9.0, and the de-Ze-MOFs adsorbent is added to the Co-containing 2+ Adsorption treatment is performed to adsorb Co 2+ The time is not less than 12 hours. The prepared Ze-MOFs material has the characteristics of low price and high adsorption capacity, and can be effectively used to treat cobalt ions in the leachate of waste ternary batteries, thereby promoting the recycling and resource recovery of waste batteries, and solving the technical problems that various adsorbents in the prior art are used to remove cobalt ions in water bodies, but have insufficient adsorption capacity, poor selectivity, slow adsorption speed and lack of environmental friendliness.
[0044] Among them, the adsorption capacity of cobalt ions by Ze-MIL-53(Al) can reach 92.67 mg / g;
[0045] The adsorption capacity of cobalt ions by Ze-MIL-53(Al)-NH2 can reach 90.80 mg / g;
[0046] The adsorption capacity of cobalt ions by Ze-MIL-53(Al)-(OH)2 can reach 73.11 mg / g.
[0047] Also, see Figure 1 , Figure 1 This is the XRD diagram of the Ze-MOFs material with cobalt ions removed according to the present invention, which, combined with relevant literature and graphs, can prove its successful preparation.
[0048] See also Figure 2 , Figure 2 This is the FT-IR image of the Ze-MOFs material with cobalt ions removed according to the present invention. The Fourier transform infrared spectrum confirms the formation of the material. 775cm -1 The Zn-MIL-53(Al) has a strong affinity to the ions at 1602 and 1440 cm-1, which is attributed to the CH bending vibration of the benzene ring. -1 The asymmetric and symmetric stretching vibrations of COO- are respectively assigned; Ze-MIL-53(Al)-NH2 at 3385cm -1 The stretching vibration of amino group is at 3400cm -1 The characteristic broad peak at is attributed to the -OH stretching vibration. The FT-IR graph can further prove the successful preparation of the material.
[0049] See also Figure 3 , Figure 3This is the SEM picture of the Ze-MOFs material with cobalt ions removed according to the present invention. It can be seen from the figure that the apparent morphology of the zeolite is irregular block-like; after Ze-MIL-53(Al), its apparent morphology becomes thicker and longer strips with a rough surface; Ze-MIL-53(Al)-NH2 presents a more regular thin strip; and Ze-MIL-53(Al)-(OH)2 presents a spherical shape with a rough surface.
[0050] See also Figure 4 , Figure 4 This is the EDS and Mapping diagram of the Ze-MOFs material for removing cobalt ions of the present invention and its raw materials. From the figure, it can be seen that the main elements contained in zeolite are O, Al, and Si, among which the O element has the highest content; and the main elements contained in the three zeolite-based MOFs are O, Al, Si, and C, and the C element has the highest content. Among them, Ze-MIL-53(Al)-NH2 has an additional N element due to the introduction of amino groups.
[0051] The present invention also provides an application of a Ze-MOFs material for separating cobalt ions in removing cobalt ions from a waste ternary lithium battery leachate, as follows:
[0052] First, take 100 mL of a cobalt-containing solution with a concentration of 10 mg / L, and adjust its pH value to between 5 and 9 using a 1.0 mol / L NaOH solution; then, add 10 mg of adsorption material, and adsorb the cobalt ions in the water at a temperature between 288.15 K and 318.15 K for a time of 0 to 24 hours.
[0053] Example 1: Please refer to Figure 5 , Figure 5 1 is a graph showing the effect of different pH values on the adsorption of cobalt ions by the Ze-MOFs material for removing cobalt ions of the present invention. In this embodiment, 100 mL of a cobalt-containing solution with a concentration of 10 mg / L was taken and adjusted to pH 8.3 using 1.0 mol / L HNO3 and NaOH solutions;
[0054] Then, 10.0 mg of adsorbent was added, and the sample was placed in a constant temperature oscillator at 298.15 K for cobalt ion adsorption treatment at an oscillation rate of 150 rpm for 12 h respectively;
[0055] After treatment, 4 mL of the solution was centrifuged at high speed (10,000 rpm, 5 minutes), and then 2 mL of the supernatant was placed in a 25 mL volumetric flask. On this basis, 1.0 mL of HAc-NaAc buffer solution with a pH of 4.5 and 1.0 mL of nitroso-R salt solution with a concentration of 4 g / L were added, and then the volume was fixed with distilled water;
[0056] Finally, the adsorption amount was measured by UV-visible spectrophotometer. The experimental results are shown in Figure 5 Among them, at pH = 8.3, the adsorption amounts of Ze-MIL-53(Al), Ze-MIL-53(Al)-NH2, and Ze-MIL-53(Al)-(OH)2 were 92.67 mg / g, 90.80 mg / g, and 73.11 mg / g, respectively.
[0057] Example 2: Please refer to Figure 6 , Figure 6 This is a result diagram of the effect of different temperatures on the adsorption of cobalt ions by Ze-MOFs materials for removing cobalt ions of the present invention; in this embodiment, 100mL of a cobalt-containing solution with a concentration of 10mg / L was taken, and it was adjusted to pH 8.3 using 1.0mol / L HNO3 and NaOH solutions. Subsequently, 10.0mg of adsorbent was added, and the sample was placed in a constant temperature oscillator at 288.15K, 298.15K, 308.15K, and 318.15K for adsorption treatment of cobalt ions, with an oscillation rate of 150rpm, and treated for 12h respectively. After treatment, 4mL of the solution was taken for high-speed centrifugation (10000rpm, 5 minutes), and then 2mL of the supernatant was taken and placed in a 25mL volumetric flask. On this basis, 1.0mL of HAc-NaAc buffer solution with a pH of 4.5 and 1.0mL of nitroso-R salt solution with a concentration of 4g / L were added, and then the volume was fixed with distilled water. Finally, the adsorption amount was measured using a UV-visible spectrophotometer. The experimental results are detailed in Figure 6 .
[0058] Embodiment 3: Figure 7 This is a result diagram of the effect of different time on the adsorption of cobalt ions by Ze-MOFs materials for removing cobalt ions of the present invention; in this embodiment, 100mL of a cobalt-containing solution with a concentration of 10mg / L was taken, and it was adjusted to pH 8.3 using 1.0mol / L HNO3 and NaOH solutions. Subsequently, 10.0mg of adsorbent was added, and the sample was placed in a 298.15K constant temperature oscillator for adsorption treatment of cobalt ions, with an oscillation rate of 150rpm, and treated for 1, 2, 4, 8, 16, and 24h, respectively. After treatment, 4mL of the solution was taken for high-speed centrifugation (10000rpm, 5 minutes), and then 2mL of the supernatant was taken and placed in a 25mL volumetric flask. On this basis, 1.0mL of HAc-NaAc buffer solution with a pH of 4.5 and 1.0mL of nitroso-R salt solution with a concentration of 4g / L were added, and then the volume was fixed with distilled water. Finally, the adsorption amount was measured using a UV-visible spectrophotometer. The experimental results are detailed in Figure 7 .
[0059] Example 4: Please refer to Figure 8 , Figure 8This is a result diagram of the effect of different cobalt ion concentrations on the adsorption of cobalt ions by Ze-MOFs materials for removing cobalt ions of the present invention; in this embodiment, 100 mL of cobalt-containing solutions with concentrations of 10, 20, 30, 40, 50, and 60 mg / L were taken, and 1.0 mol / L of HNO3 and NaOH solutions were used to adjust the pH to 8.3, and then 10.0 mg of adsorbent was added. The sample was then oscillated at 150 rpm for 12.0 hours in a 298.15K constant temperature oscillator, and then 4 mL of the solution was taken for high-speed centrifugation (10000 rpm, 5 minutes). Next, 2 mL of the supernatant was taken in a 25 mL volumetric flask, 1.0 mL of HAc-NaAc buffer solution with a pH of 4.5 and 1.0 mL of nitroso-R salt solution with a concentration of 4 g / L were added, and the volume was fixed with distilled water. Finally, the adsorption amount was measured using a UV-visible spectrophotometer. The experimental results are detailed in Figure 8 shown.
[0060] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.
Claims
1. A Ze-MOFs material for cobalt ion separation, characterized in that: Including zeolite, terephthalic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid.
2. A method for preparing a Ze-MOFs material for cobalt ion separation, for preparing the Ze-MOFs material for cobalt ion separation as claimed in claim 1, characterized in that: The steps include: Step 1: Activation of artificial zeolite: Place the zeolite in a crucible, place it in a muffle furnace for activation, and then cool it to room temperature; Step 2: crushing the artificial zeolite: grinding the cooled zeolite in a ball mill, and collecting the powder after grinding; Step 3: First, disperse the powdered zeolite and organic ligand into deionized water, stir them thoroughly at room temperature to evenly disperse the zeolite and organic ligand, then add acetic acid, transfer them into a hydrothermal reactor with polytetrafluoroethylene for reaction, recover the material after the reaction is completed, wash the material with deionized water 2-3 times, and vacuum dry it to obtain Ze-MOFs material for cobalt ion separation.
3. The method for preparing the Ze-MOFs material for cobalt ion separation according to claim 2, characterized in that: In step 1, the zeolite is placed in a crucible and placed in a muffle furnace at an activation temperature of 800° C. for 10 hours.
4. The method for preparing the Ze-MOFs material for cobalt ion separation according to claim 3, characterized in that: In step 2, the grinding rate is 320 rpm and the grinding time is 5 h.
5. The method for preparing the Ze-MOFs material for cobalt ion separation according to claim 4, characterized in that: In step three, the reaction temperature in the hydrothermal reactor is 120° C. and the reaction time is 24 h.
6. The method for preparing the Ze-MOFs material for cobalt ion separation according to claim 5, characterized in that: In step three, after the reaction in the hydrothermal reactor is completed, the material is recovered by centrifugal separation.
7. The method for preparing the Ze-MOFs material for cobalt ion separation according to claim 6, characterized in that: The organic ligands include terephthalic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid.
8. The method for preparing the Ze-MOFs material for cobalt ion separation according to claim 7, characterized in that: The Ze-MOFs material is one of Ze-MIL-53(Al), Ze-MIL-53(Al)-NH2, and Ze-MIL-53(Al)-(OH)2.
Citation Information
Patent Citations
Metal organic skeleton material for removing cobalt ions from wastewater and preparation method of metal organic skeleton material
CN106861627A
MS-MIL-53-PAN material for removing cobalt ions in wastewater and preparation method of MS-MIL-53-PAN material
CN117680111A
Double-framework MOFs material MS-MIL-101 (Al) for cobalt ion separation and preparation method of double-framework MOFs material MS-MIL-101 (Al)
CN117757104A
MOFs-loaded zeolite molecular sieve composite material as well as preparation method and application thereof
CN118356913A