Salicylic acid molecularly imprinted adsorption material and preparation method thereof
By using the synergistic effect of zeolite molecular sieve, modifier and crosslinking agent in molecular imprinting technology, an efficient salicylic acid molecular imprinting adsorption material was prepared, which solved the low efficiency and selection of salicylic acid removal process in the prior art in the process of salicylic acid in the prior art The poor performance problem has achieved efficient and green separation and purification and good reuse performance.
Patent Information
- Application Number
- CN202411176961.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art has problems such as complex operation, high cost, low efficiency and poor selectivity when removing salicylic acid and its impurities, and it is difficult to meet increasingly stringent environmental protection requirements, especially in the detection and enrichment of low-concentration pollutants.
Using molecular imprinting technology, the synergistic effect of zeolite molecular sieve as matrix material and specific modifiers and crosslinking agents is prepared to produce salicylic acid molecular imprinting adsorption materials with high adsorption capacity and selectivity, using specific chemical reactions and physical structures. Design and create blotting sites that match salicylic acid molecules, improve adsorption selectivity and enhance mechanical strength and chemical stability.
It significantly improves the adsorption selectivity and adsorption capacity of salicylic acid, achieves efficient separation and purification, reduces environmental pollution in the production process, meets the high standards of the green chemistry and pharmaceutical industry, and has good reusability.
Smart Images

Figure BDA0005010971320000121 
Figure BDA0005010971320000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of molecular imprinting blended membranes, in particular to a salicylic acid molecular imprinting adsorption material and a preparation method thereof. Background Art
[0002] Salicylic acid (SA), also known as o-hydroxybenzoic acid, is an important organic compound that is widely used in chemical, pharmaceutical, cosmetic and other fields. However, impurities that may be produced during the production and use of salicylic acid not only affect product quality, but also pose potential risks to human health and the environment.
[0003] Hydroxybenzoic acid compounds have attracted much attention in many fields such as chemistry, medicine, food additives and environmental monitoring due to their unique biological activity and wide application. However, the presence of these compounds also brings about environmental pollution and health risks, especially their discharge in industrial wastewater, which has become an environmental problem that needs to be solved urgently.
[0004] Traditional treatment methods, such as adsorption, extraction, membrane separation, etc., can remove these pollutants to a certain extent, but they usually have problems such as complex operation, high cost, low efficiency or poor selectivity. Especially for the detection and enrichment of low-concentration pollutants, existing technologies are difficult to meet the increasingly stringent environmental protection requirements.
[0005] As a new separation and recognition technology, molecular imprinting technology provides new possibilities for solving the above problems due to its high selectivity, high stability and reusability. This technology forms a stable complex with a template molecule through a specific functional monomer, and prepares a polymer with a specific recognition site through a polymerization reaction. After removing the template molecule, the imprinted pores left in the polymer can specifically recognize and adsorb the target molecule.
[0006] Given the advantages of molecular imprinting technology in specific molecular recognition and adsorption, its application prospects in environmental monitoring and pollutant treatment are broad. By developing new molecular imprinting materials, the separation and purification efficiency of salicylic acid and its impurities can be effectively improved, while the detection and enrichment capabilities of parahydroxybenzoic acid compounds can be enhanced to meet the challenges of environmental pollution and health risks.
[0007] China's invention patent CN102698721B discloses a method for preparing a surface imprinted adsorbent for separating salicylic acid from wastewater, specifically a method for preparing a surface imprinted adsorbent for salicylic acid by a precipitation polymerization process using wollastonite as a substrate, salicylic acid (SA) as a template molecule, acrylamide (AM) as a functional monomer, ethylene glycol di(methacrylate) ester (EGDMA) as a crosslinker, and 2,2'-azobisisobutyronitrile (AIBN) as an initiator. The results show that the surface imprinted adsorbent for salicylic acid obtained by the invention has a high adsorption capacity, fast adsorption kinetics, and obvious recognition performance of salicylic acid molecules. However, the adsorption effect of the imprinted adsorbent prepared by the invention is not ideal, and the reusability is poor. Summary of the invention
[0008] In view of the defects of the prior art, the present invention aims to develop a new type of salicylic acid molecular imprinting adsorption material, which improves the selective adsorption capacity of salicylic acid by optimizing the molecular imprinting technology, and realizes efficient and green separation and purification of salicylic acid. The invention can not only improve the purity of salicylic acid products, but also help reduce environmental pollution in the production process, meeting the high standards of modern green chemistry and pharmaceutical industries.
[0009] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0010] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows, in parts by weight:
[0011] Step 1, reflux 10-20 zeolite molecular sieve with 400-600 parts of 2-4 mol / L phosphoric acid solution, then wash with water until neutral, and dry at 60-80° C. to obtain a pretreated product;
[0012] Step 2, dispersing the pretreated material prepared in step 1 in 400-600 parts of n-hexane, adding 150-250 parts of 3-methacryloxypropyltri(isopropyleneoxy)silane, reacting at 60-80° C. for 5-24 hours, then washing with methanol and water respectively, and vacuum drying at 60-80° C. for 5-24 hours to obtain a modified material;
[0013] Step 3, 4 to 8 parts of polyether ketone, 200 to 300 parts of dichloromethane, 100 to 150 parts of chlorosulfonic acid, and 1000 to 1500 parts of anhydrous ethanol are mixed for 1 to 3 hours, and vacuum dried at 60 to 80° C. to constant weight to obtain a treating agent;
[0014] Step 4, adding 10 to 20 parts of salicylic acid and 30 to 50 parts of acrylamide to 400 to 600 parts of solvent, introducing nitrogen to exhaust oxygen, and standing at 3 to 8° C. for 2 to 10 hours to obtain a preassembled system;
[0015] Step 5, adding 400-600 parts of trimethylolpropane triacrylate, the modified material obtained in step 2 and 0.3-0.5 parts of initiator, as well as the treating agent obtained in step 3 and 8-12 parts of quaternary ammonium salt into the preassembled system, reacting at 60-80° C. for 10-30 hours to obtain a mixture; degassing the mixture, then casting a film, immersing it in water for 30-50 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing to remove the template molecule salicylic acid, and then washing with methanol for 1-3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0016] In the step 1, the reflux temperature is 60-80° C. and the reflux time is 5-24 hours.
[0017] The vacuum drying is carried out at 60 to 80° C. for 5 to 24 hours.
[0018] The initiator is dibenzoyl peroxide.
[0019] The quaternary ammonium salt is formylmethyltrimethylammonium chloride.
[0020] The solvent is one of acetonitrile and dimethyl sulfoxide.
[0021] The degassing step is to place the mixture at 30 to 50° C. for 20 to 40 hours for degassing.
[0022] The film casting temperature is 30-50°C.
[0023] The volume ratio of methanol to acetic acid is 8-10:1.
[0024] In the preparation method of the salicylic acid molecular imprinting adsorption material of the present invention, the functions of each substance are as follows:
[0025] Zeolite molecular sieve is used as a matrix material. Due to its porous structure and high specific surface area, zeolite molecular sieve provides a large number of active sites, which is conducive to the formation of molecular imprinting and the improvement of adsorption performance.
[0026] Phosphoric acid solution is used to pretreat zeolite molecular sieves. Phosphoric acid can be used as a modifier to enhance the surface activity and stability of zeolite molecular sieves.
[0027] Normal hexane is used as a solvent to disperse the pretreated zeolite molecular sieve to ensure that the modifier can evenly contact and react with the zeolite molecular sieve.
[0028] 3-Methacryloxypropyltri(isopropenyloxy)silane is used as a modifier to react with the functional groups on the surface of the zeolite molecular sieve to form a stable chemical bond, thereby enhancing the hydrophilicity and mechanical strength of the material.
[0029] As the main component in the preparation of the treating agent, polyetherketone may help improve the film-forming property and durability of the final product due to its good chemical and thermal stability.
[0030] Substances such as dichloromethane, chlorosulfonic acid, and anhydrous ethanol are mixed with polyetherketone to prepare treating agents, which may involve sulfonation reactions to increase the hydrophilicity of the material or serve as solvents and reaction media.
[0031] Acrylamide, as a functional monomer, forms a pre-assembled system with salicylic acid and participates in the polymerization reaction to form a molecular imprinting structure.
[0032] Acetonitrile is used as a solvent to dissolve acrylamide and salicylic acid to form a pre-assembled system.
[0033] Trimethylolpropane triacrylate acts as a crosslinking agent and reacts with other components to form a three-dimensional network structure, thereby enhancing the mechanical strength and stability of the adsorption material.
[0034] Benzoyl peroxide acts as an initiator for polymerization reactions, promoting the polymerization of monomers such as acrylamide.
[0035] Formyltrimethylammonium chloride is a quaternary ammonium salt with both hydrophilic and lipophilic properties, which enables it to increase the viscosity in the casting solution and improve the film-forming rate during the phase transformation membrane-making process, thereby helping to form a more ordered pore structure inside the membrane.
[0036] The methanol and acetic acid mixture is used to remove the template molecule salicylic acid, methanol is used to wash the adsorbent material to remove the residual template molecules or other soluble impurities, and acetic acid helps to destroy hydrogen bonds and promote the removal of template molecules.
[0037] Through the synergistic effect of these substances, the present invention successfully prepares salicylic acid molecular imprinting adsorption materials with high adsorption capacity and selectivity.
[0038] Compared with the prior art, it has the following beneficial effects:
[0039] 1) The present invention adopts molecular imprinting technology, and through specific chemical reactions and physical structure design, creates imprinting sites in the adsorption material that match the molecular structure of salicylic acid, significantly improving the adsorption selectivity of salicylic acid, and can effectively selectively adsorb target molecules from complex samples containing a variety of impurities with similar structures.
[0040] 2) The zeolite molecular sieve matrix, specific modifier and cross-linking agent selected in the present invention work together to improve the adsorption capacity and adsorption rate of the adsorption material, while maintaining good mechanical strength and chemical stability, so that the adsorption material exhibits high adsorption efficiency and long service life in practical applications.
[0041] 3) After a specific post-treatment and template molecule removal process, the adsorption material prepared by the present invention has good regeneration characteristics, allowing for repeated use in the adsorption-desorption cycle, reducing material consumption, lowering long-term operating costs, and reducing waste generation, meeting the requirements of green chemistry and sustainable development. DETAILED DESCRIPTION
[0042] Main sources of substances:
[0043] Zeolite molecular sieve: purchased from Shanghai Youxin Molecular Sieve Co., Ltd., particle size 3-5mm;
[0044] 3-Methacryloyloxypropyltri(isopropenyloxy)silane: CAS No.: 78051-94-2;
[0045] Polyetherketone: purchased from Victrex, UK, brand name ST;
[0046] Trimethylolpropane triacrylate: CAS number: 15625-89-5.
[0047] γ-Aminopropyltriethoxysilane: CAS number: 919-30-2.
[0048] Methacrylate propoxytriacetoxysilane: CAS number: 51772-85-1.
[0049] Glycidyl methacrylate: CAS number: 106-91-2.
[0050] Ethylene glycol dimethacrylate: CAS number: 97-90-5.
[0051] The remaining raw materials in the examples and comparative examples of the present invention are all commercially available products.
[0052] The design idea of the present invention is to develop an efficient salicylic acid molecular imprinting adsorption material for selectively adsorbing and enriching salicylic acid from complex samples. In order to achieve this goal, the present invention adopts a porous inorganic material (such as a zeolite molecular sieve) as a matrix to increase adsorption sites and provide the physical structure required for molecular imprinting. By selecting a suitable modifier (such as 3-methacryloxypropyl tri(isopropyleneoxy)silane) to chemically modify the matrix surface, the stability and hydrophilicity of the material in the organic medium are enhanced, and the specific interaction with the target molecule is promoted. In addition, by carefully selecting a cross-linking agent (such as trimethylolpropane triacrylate) to construct a three-dimensional network structure, not only the mechanical strength and chemical stability of the material are enhanced, but also the pore characteristics of the adsorption material are optimized, thereby improving the adsorption capacity and selectivity of salicylic acid. The entire design idea embodies the cross-fusion of material science, chemical engineering and molecular recognition technology, and aims to achieve efficient separation and enrichment of specific target molecules through molecular imprinting technology.
[0053] Example 1
[0054] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows:
[0055] Step 1, 15g of zeolite molecular sieve was refluxed at 70°C for 12 hours with 500g of 3.0mol / L phosphoric acid solution, then washed with water until neutral, and dried at 70°C to obtain a pretreated product;
[0056] Step 2, dispersing the pretreated material prepared in step 1 in 500 g of n-hexane, adding 200 g of 3-methacryloxypropyltri(isopropenyloxy)silane, reacting at 70° C. for 10 hours, then washing with methanol and water respectively, and vacuum drying at 70° C. for 12 hours to obtain a modified material;
[0057] Step 3, 6 g of polyether ketone, 250 g of dichloromethane, 120 g of chlorosulfonic acid, and 1200 g of anhydrous ethanol were mixed for 2 hours, and vacuum dried at 70° C. to constant weight to obtain a treating agent;
[0058] Step 4, add 15 g of salicylic acid and 40 g of acrylamide to 500 g of acetonitrile, introduce nitrogen to exhaust oxygen, and let stand at 5° C. for 5 hours to obtain a preassembled system;
[0059] Step 5, adding 500g of trimethylolpropane triacrylate, the modified material obtained in step 2 and 0.4g of dibenzoyl peroxide, as well as the treating agent obtained in step 3 and 10g of formylmethyltrimethylammonium chloride to the preassembled system, reacting at 70°C for 20 hours to obtain a mixture; standing the mixture at 40°C for 30 hours to degas, then casting a film at 40°C, immersing in water for 40 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing, the volume ratio of methanol to acetic acid is 9:1, removing the template molecule salicylic acid, and then washing with methanol for 3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0060] Example 2
[0061] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows:
[0062] Step 1, 15g of montmorillonite is refluxed at 70°C for 12 hours with 500g of 3.0mol / L phosphoric acid solution, the montmorillonite particle size is 10-20μm, then washed with water to neutrality, and dried at 70°C to obtain a pretreated product;
[0063] Step 2, dispersing the pretreated material prepared in step 1 in 500 g of n-hexane, adding 200 g of 3-methacryloxypropyltri(isopropenyloxy)silane, reacting at 70° C. for 10 hours, then washing with methanol and water respectively, and vacuum drying at 70° C. for 12 hours to obtain a modified material;
[0064] Step 3, 6 g of polyether ketone, 250 g of dichloromethane, 120 g of chlorosulfonic acid, and 1200 g of anhydrous ethanol were mixed for 2 hours, and vacuum dried at 70° C. to constant weight to obtain a treating agent;
[0065] Step 4, add 15 g of salicylic acid and 40 g of acrylamide to 500 g of acetonitrile, introduce nitrogen to exhaust oxygen, and let stand at 5° C. for 5 hours to obtain a preassembled system;
[0066] Step 5, adding 500g of trimethylolpropane triacrylate, the modified material obtained in step 2 and 0.4g of dibenzoyl peroxide, as well as the treating agent obtained in step 3 and 10g of formylmethyltrimethylammonium chloride to the preassembled system, reacting at 70°C for 20 hours to obtain a mixture; standing the mixture at 40°C for 30 hours to degas, then casting a film at 40°C, immersing in water for 40 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing, the volume ratio of methanol to acetic acid is 9:1, removing the template molecule salicylic acid, and then washing with methanol for 3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0067] Example 3
[0068] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows:
[0069] Step 1, 15g of aluminum oxide is refluxed with 500g of 3.0mol / L phosphoric acid solution at 70°C for 12 hours, the particle size of the aluminum oxide is 0.5-4μm, then washed with water to neutrality, and dried at 70°C to obtain a pretreated product;
[0070] Step 2, dispersing the pretreated material prepared in step 1 in 500 g of n-hexane, adding 200 g of 3-methacryloxypropyltri(isopropenyloxy)silane, reacting at 70° C. for 10 hours, then washing with methanol and water respectively, and vacuum drying at 70° C. for 12 hours to obtain a modified material;
[0071] Step 3, 6 g of polyether ketone, 250 g of dichloromethane, 120 g of chlorosulfonic acid, and 1200 g of anhydrous ethanol were mixed for 2 hours, and vacuum dried at 70° C. to constant weight to obtain a treating agent;
[0072] Step 4, add 15 g of salicylic acid and 40 g of acrylamide to 500 g of acetonitrile, introduce nitrogen to exhaust oxygen, and let stand at 5° C. for 5 hours to obtain a preassembled system;
[0073] Step 5, adding 500g of trimethylolpropane triacrylate, the modified material obtained in step 2 and 0.4g of dibenzoyl peroxide, as well as the treating agent obtained in step 3 and 10g of formylmethyltrimethylammonium chloride to the preassembled system, reacting at 70°C for 20 hours to obtain a mixture; standing the mixture at 40°C for 30 hours to degas, then casting a film at 40°C, immersing in water for 40 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing, the volume ratio of methanol to acetic acid is 9:1, removing the template molecule salicylic acid, and then washing with methanol for 3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0074] Example 4
[0075] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows:
[0076] Step 1, 15g of wollastonite is refluxed with 500g of 3.0mol / L phosphoric acid solution at 70°C for 12 hours, the wollastonite particle size is 5-20μm, then washed with water to neutrality, and dried at 70°C to obtain a pretreated product;
[0077] Step 2, dispersing the pretreated material prepared in step 1 in 500 g of n-hexane, adding 200 g of 3-methacryloxypropyltri(isopropenyloxy)silane, reacting at 70° C. for 10 hours, then washing with methanol and water respectively, and vacuum drying at 70° C. for 12 hours to obtain a modified material;
[0078] Step 3, 6 g of polyether ketone, 250 g of dichloromethane, 120 g of chlorosulfonic acid, and 1200 g of anhydrous ethanol were mixed for 2 hours, and vacuum dried at 70° C. to constant weight to obtain a treating agent;
[0079] Step 4, add 15 g of salicylic acid and 40 g of acrylamide to 500 g of acetonitrile, introduce nitrogen to exhaust oxygen, and let stand at 5° C. for 5 hours to obtain a preassembled system;
[0080] Step 5, adding 500g of trimethylolpropane triacrylate, the modified material obtained in step 2 and 0.4g of dibenzoyl peroxide, as well as the treating agent obtained in step 3 and 10g of formylmethyltrimethylammonium chloride to the preassembled system, reacting at 70°C for 20 hours to obtain a mixture; standing the mixture at 40°C for 30 hours to degas, then casting a film at 40°C, immersing in water for 40 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing, the volume ratio of methanol to acetic acid is 9:1, removing the template molecule salicylic acid, and then washing with methanol for 3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0081] Example 5
[0082] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows:
[0083] Step 1, 15g of zeolite molecular sieve was refluxed at 70°C for 12 hours with 500g of 3.0mol / L phosphoric acid solution, then washed with water until neutral, and dried at 70°C to obtain a pretreated product;
[0084] Step 2, dispersing the pretreated material prepared in step 1 in 500 g of n-hexane, adding 200 g of γ-aminopropyltriethoxysilane, reacting at 70° C. for 10 hours, then washing with methanol and water respectively, and vacuum drying at 70° C. for 12 hours to obtain a modified material;
[0085] Step 3, 6 g of polyether ketone, 250 g of dichloromethane, 120 g of chlorosulfonic acid, and 1200 g of anhydrous ethanol were mixed for 2 hours, and vacuum dried at 70° C. to constant weight to obtain a treating agent;
[0086] Step 4, add 15 g of salicylic acid and 40 g of acrylamide to 500 g of acetonitrile, introduce nitrogen to exhaust oxygen, and let stand at 5° C. for 5 hours to obtain a preassembled system;
[0087] Step 5, adding 500g of trimethylolpropane triacrylate, the modified material obtained in step 2 and 0.4g of dibenzoyl peroxide, as well as the treating agent obtained in step 3 and 10g of formylmethyltrimethylammonium chloride to the preassembled system, reacting at 70°C for 20 hours to obtain a mixture; standing the mixture at 40°C for 30 hours to degas, then casting a film at 40°C, immersing in water for 40 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing, the volume ratio of methanol to acetic acid is 9:1, removing the template molecule salicylic acid, and then washing with methanol for 3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0088] Example 6
[0089] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows:
[0090] Step 1, 15g of zeolite molecular sieve was refluxed at 70°C for 12 hours with 500g of 3.0mol / L phosphoric acid solution, then washed with water until neutral, and dried at 70°C to obtain a pretreated product;
[0091] Step 2, dispersing the pretreated material prepared in step 1 in 500 g of n-hexane, adding 200 g of methacrylate propoxytriacetoxysilane, reacting at 70° C. for 10 hours, then washing with methanol and water respectively, and vacuum drying at 70° C. for 12 hours to obtain a modified material;
[0092] Step 3, 6 g of polyether ketone, 250 g of dichloromethane, 120 g of chlorosulfonic acid, and 1200 g of anhydrous ethanol were mixed for 2 hours, and vacuum dried at 70° C. to constant weight to obtain a treating agent;
[0093] Step 4, add 15 g of salicylic acid and 40 g of acrylamide to 500 g of acetonitrile, introduce nitrogen to exhaust oxygen, and let stand at 5° C. for 5 hours to obtain a preassembled system;
[0094] Step 5, adding 500g of trimethylolpropane triacrylate, the modified material obtained in step 2 and 0.4g of dibenzoyl peroxide, as well as the treating agent obtained in step 3 and 10g of formylmethyltrimethylammonium chloride to the preassembled system, reacting at 70°C for 20 hours to obtain a mixture; standing the mixture at 40°C for 30 hours to degas, then casting a film at 40°C, immersing in water for 40 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing, the volume ratio of methanol to acetic acid is 9:1, removing the template molecule salicylic acid, and then washing with methanol for 3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0095] Example 7
[0096] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows:
[0097] Step 1, 15g of zeolite molecular sieve was refluxed at 70°C for 12 hours with 500g of 3.0mol / L phosphoric acid solution, then washed with water until neutral, and dried at 70°C to obtain a pretreated product;
[0098] Step 2, dispersing the pretreated material prepared in step 1 in 500 g of n-hexane, adding 200 g of 3-methacryloxypropyltri(isopropenyloxy)silane, reacting at 70° C. for 10 hours, then washing with methanol and water respectively, and vacuum drying at 70° C. for 12 hours to obtain a modified material;
[0099] Step 3, 6 g of polyether ketone, 250 g of dichloromethane, 120 g of chlorosulfonic acid, and 1200 g of anhydrous ethanol were mixed for 2 hours, and vacuum dried at 70° C. to constant weight to obtain a treating agent;
[0100] Step 4, add 15 g of salicylic acid and 40 g of acrylamide to 500 g of acetonitrile, introduce nitrogen to exhaust oxygen, and let stand at 5° C. for 5 hours to obtain a preassembled system;
[0101] Step 5, adding 500g of glycidyl methacrylate, the modified material obtained in step 2 and 0.4g of dibenzoyl peroxide, as well as the treating agent obtained in step 3 and 10g of formylmethyltrimethylammonium chloride to the preassembled system, reacting at 70°C for 20 hours to obtain a mixture; standing the mixture at 40°C for 30 hours to degas, then casting a film at 40°C, immersing in water for 40 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing, the volume ratio of methanol to acetic acid is 9:1, removing the template molecule salicylic acid, and then washing with methanol for 3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0102] Example 8
[0103] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows:
[0104] Step 1, 15g of zeolite molecular sieve was refluxed at 70°C for 12 hours with 500g of 3.0mol / L phosphoric acid solution, then washed with water until neutral, and dried at 70°C to obtain a pretreated product;
[0105] Step 2, dispersing the pretreated material prepared in step 1 in 500 g of n-hexane, adding 200 g of 3-methacryloxypropyltri(isopropenyloxy)silane, reacting at 70° C. for 10 hours, then washing with methanol and water respectively, and vacuum drying at 70° C. for 12 hours to obtain a modified material;
[0106] Step 3, 6 g of polyether ketone, 250 g of dichloromethane, 120 g of chlorosulfonic acid, and 1200 g of anhydrous ethanol were mixed for 2 hours, and vacuum dried at 70° C. to constant weight to obtain a treating agent;
[0107] Step 4, add 15 g of salicylic acid and 40 g of acrylamide to 500 g of acetonitrile, introduce nitrogen to exhaust oxygen, and let stand at 5° C. for 5 hours to obtain a preassembled system;
[0108] Step 5, adding 500g of ethylene glycol dimethacrylate, the modified material obtained in step 2 and 0.4g of dibenzoyl peroxide, as well as the treating agent obtained in step 3 and 10g of formylmethyltrimethylammonium chloride into the preassembled system, reacting at 70°C for 20 hours to obtain a mixture; standing the mixture at 40°C for 30 hours to degas, then casting a film at 40°C, immersing in water for 40 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing, the volume ratio of methanol to acetic acid is 9:1, removing the template molecule salicylic acid, and then washing with methanol for 3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0109] Comparative Example 1
[0110] A method for preparing a salicylic acid molecular imprinting adsorption material is as follows:
[0111] Step 1, add 15g of salicylic acid and 40g of acrylamide to 500g of acetonitrile, introduce nitrogen to exhaust oxygen, and let stand at 5°C for 5 hours to obtain a preassembled system;
[0112] Step 2: Add 500g of trimethylolpropane triacrylate, 0.4g of dibenzoyl peroxide and 10g of formylmethyltrimethylammonium chloride to the preassembled system, react at 70°C for 20 hours to obtain a mixture; let the mixture stand at 40°C for 30 hours to degas, then cast a film at 40°C, immerse in water for 40 minutes and then take out; use a mixed solution of methanol and acetic acid as an extract for washing, the volume ratio of methanol to acetic acid is 9:1, remove the template molecule salicylic acid, and then wash with methanol for 3 times to obtain a salicylic acid molecular imprinting adsorption material.
[0113] Test Example 1
[0114] Adsorption performance test
[0115] 10 mL of salicylic acid solutions with initial concentrations of 25, 60, 80, 150, 200, 250, 300, 350 and 400 mg / L were added to colorimetric tubes, and 20 mg of the salicylic acid molecular imprinting adsorption material prepared by the present invention was added respectively. The test solution was placed in a water bath at 25° C. and allowed to stand for 12 h, and then centrifuged to obtain a supernatant. The concentration of unadsorbed salicylic acid molecules was determined by ultraviolet spectroscopy, and the adsorption capacity was calculated based on the result.
[0116] The test results are shown in Table 1.
[0117] Table 1
[0118] Experimental protocol Saturated adsorption capacity (mg / g) Example 1 84.21 Example 2 76.84 Example 3 74.98 Example 4 75.59 Example 5 80.47 Example 6 81.41 Example 7 81.27 Example 8 80.12 Comparative Example 1 71.57
[0119] Test Example 2
[0120] Reuse experiment
[0121] Take 3.0mL of 0.5mg / ml p-hydroxybenzoic acid aqueous solution, add 20mg of salicylic acid molecular imprinting adsorption material prepared by the present invention, shake at 25℃ for 2h, after adsorption, use acetonitrile to wash away the surface adsorption by magnetic separation, and then use a mixture of methanol and acetic acid (9:1, V / V) to elute until the p-hydroxybenzoic acid is removed, finally wash the particles with methanol to neutrality, and vacuum dry the desorbed material at 50℃ to constant weight. Repeat the same adsorption-desorption process 5 times, calculate the adsorption reduction rate, and evaluate the reuse effect.
[0122] The test results are shown in Table 2.
[0123] Table 2
[0124]
[0125]
[0126] It can be seen from the data in Table 1 and Table 2 that the salicylic acid molecular imprinting adsorption material prepared in Example 1 has a higher saturated adsorption capacity and better reuse effect.
[0127] Embodiment 1 of the present invention adopts zeolite molecular sieve as matrix material, and is superior to the montmorillonite of embodiment 2, the alumina of embodiment 3 and the wollastonite of embodiment 4 in the performance of adsorbing salicylic acid, and the reason may be attributed to the unique properties of zeolite molecular sieve and the advantages in the preparation process. Zeolite molecular sieve has a highly ordered pore structure and a high specific surface area, which provides more effective adsorption sites for salicylic acid molecules, thereby increasing the adsorption capacity. At the same time, the pore size and shape of zeolite molecular sieve may be more matched with the structural characteristics of salicylic acid molecules, which is conducive to the formation of specific recognition sites in the molecular imprinting process. In addition, the performance of zeolite molecular sieve in chemical and thermal stability, and the interaction with the modifier in the surface modification step, may further improve the selectivity and adsorption efficiency of the adsorbent material. These comprehensive factors make the zeolite molecular sieve matrix of embodiment 1 surpass the materials used in other embodiments in adsorption performance.
[0128] In Example 1 of the present invention, 3-methacryloxypropyl tri(isopropenyloxy)silane is selected as a modifier, which may provide better performance due to its unique chemical structure compared to γ-aminopropyl triethoxysilane in Example 5 and methacrylic acid propoxy triacetoxysilane in Example 6. The three isopropenyloxy groups contained in 3-methacryloxypropyl tri(isopropenyloxy)silane may enhance the grafting reaction with the surface of the zeolite molecular sieve, thereby forming a more uniform and stable modified layer on the surface of the zeolite molecular sieve. This modified layer not only improves the hydrophilicity of the matrix, but also may enhance the adsorption capacity of salicylic acid molecules by forming more hydrogen bonding points. At the same time, the long chain structure of 3-methacryloxypropyl may provide better spatial matching and flexibility for the imprinted layer, which helps to improve the selectivity and adsorption efficiency of the adsorbent material. Therefore, the use of this modifier may create more effective binding sites in the molecular imprinting process, thereby improving the adsorption capacity and selectivity of salicylic acid, which is manifested as a higher saturated adsorption capacity and a lower adsorption reduction rate in the adsorption performance test.
[0129] In Example 1 of the present invention, trimethylolpropane triacrylate is used as a cross-linking agent. In the process of preparing salicylic acid molecular imprinting adsorption material, compared with glycidyl methacrylate in Example 7 and ethylene glycol dimethacrylate in Example 8, it may provide better performance due to its unique three-dimensional multi-functional structure. Trimethylolpropane triacrylate contains three acrylate functional groups, which not only increases the cross-linking density of the polymer network, but also may enhance the interaction with the zeolite molecular sieve matrix, thereby improving the mechanical stability and chemical stability of the adsorption material. In addition, the cross-linked network formed by trimethylolpropane triacrylate during the polymerization process may have a more suitable pore size and pore structure, providing more effective adsorption sites and better molecular recognition ability for salicylic acid molecules. The combined effect of these characteristics makes the adsorption material with trimethylolpropane triacrylate as a cross-linking agent perform better in terms of adsorption capacity and selectivity, thereby showing higher adsorption efficiency and better reusability in practical applications.
[0130] In embodiment 1, zeolite molecular sieve is used as matrix material, because of its porous structure and high specific surface area, a large number of active sites are provided for adsorption and molecular imprinting. 3-methacryloxypropyl tri (isopropyleneoxy) silane is used as modifier, and covalent bonding occurs with zeolite molecular sieve surface through its silane structure, enhances the stability of molecular sieve in organic medium, and may participate in subsequent reactions through its acryloyloxy group. Trimethylolpropane triacrylate is used as cross-linking agent, and its acrylate functional group forms a cross-linked network with other monomers and modifiers during polymerization, thereby improving the mechanical strength and chemical stability of adsorbent material. This interaction not only enhances the adsorption performance of the material, but also realizes the highly selective recognition of salicylic acid molecules through molecular imprinting technology, thereby preparing salicylic acid molecular imprinting adsorption material with excellent adsorption capacity and reusability.
Claims
1. A method for preparing a salicylic acid molecular imprinting adsorption material, characterized in that: The method is as follows, in parts by weight: Step 1, reflux 10-20 zeolite molecular sieve with 400-600 parts of 2-4 mol / L phosphoric acid solution, then wash with water until neutral, and dry at 60-80° C. to obtain a pretreated product; Step 2, dispersing the pretreated material prepared in step 1 in 400-600 parts of n-hexane, adding 150-250 parts of 3-methacryloxypropyltri(isopropyleneoxy)silane, reacting at 60-80° C. for 5-24 hours, then washing with methanol and water respectively, and vacuum drying at 60-80° C. for 5-24 hours to obtain a modified material; Step 3, 4 to 8 parts of polyether ketone, 200 to 300 parts of dichloromethane, 100 to 150 parts of chlorosulfonic acid, and 1000 to 1500 parts of anhydrous ethanol are mixed for 1 to 3 hours, and vacuum dried at 60 to 80° C. to constant weight to obtain a treating agent; Step 4, adding 10 to 20 parts of salicylic acid and 30 to 50 parts of acrylamide to 400 to 600 parts of solvent, introducing nitrogen to exhaust oxygen, and standing at 3 to 8° C. for 2 to 10 hours to obtain a preassembled system; Step 5, adding 400-600 parts of trimethylolpropane triacrylate, the modified material obtained in step 2 and 0.3-0.5 parts of initiator, as well as the treating agent obtained in step 3 and 8-12 parts of quaternary ammonium salt into the preassembled system, reacting at 60-80° C. for 10-30 hours to obtain a mixture; degassing the mixture, then casting a film, immersing it in water for 30-50 minutes and then taking it out; using a mixed solution of methanol and acetic acid as an extracting solution for washing to remove the template molecule salicylic acid, and then washing with methanol for 1-3 times to obtain a salicylic acid molecular imprinting adsorption material.
2. The method for preparing the salicylic acid molecularly imprinted adsorption material according to claim 1, characterized in that: In the step 1, the reflux temperature is 60 to 80° C. and the reflux time is 5 to 24 hours.
3. The method for preparing the salicylic acid molecularly imprinted adsorption material according to claim 1, characterized in that: The vacuum drying is carried out at 60 to 80° C. for 5 to 24 hours.
4. The method for preparing the salicylic acid molecularly imprinted adsorption material according to claim 1, characterized in that: The initiator is dibenzoyl peroxide.
5. The method for preparing the salicylic acid molecularly imprinted adsorption material according to claim 1, characterized in that: The quaternary ammonium salt is formylmethyltrimethylammonium chloride.
6. The method for preparing the salicylic acid molecularly imprinted adsorption material according to claim 1, characterized in that: The solvent is one of acetonitrile and dimethyl sulfoxide.
7. The method for preparing the salicylic acid molecularly imprinted adsorption material according to claim 1, characterized in that: The degassing step is to place the mixture at 30 to 50° C. for 20 to 40 hours for degassing.
8. The method for preparing the salicylic acid molecularly imprinted adsorption material according to claim 1, characterized in that: The film casting temperature is 30-50°C.
9. The method for preparing the salicylic acid molecularly imprinted adsorption material according to claim 1, characterized in that: The volume ratio of methanol to acetic acid is 8-10:
1.
10. A salicylic acid molecular imprinting adsorption material, characterized in that: The method is prepared by any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method for adsorbent for separating salicylic acid surface imprint from waste water
CN102698721B