Lanthanum ferrite catalyst with lanthanum defect, preparation method of lanthanum ferrite catalyst and application of lanthanum ferrite catalyst in photocatalytic degradation of plastic

Through the lanthanum-deficient lanthanum ferrite catalyst, electrons and holes are generated in the photocatalytic system, the problem of microplastics being difficult to degrade is solved, and efficient removal and resource conversion is achieved, especially the degradation rate of polyethylene is increased by nearly 4 times. Suitable for applications in complex water environments.

CN118976503AActive Publication Date: 2024-11-19SHANXI UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411043901.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The prior art cannot effectively convert microplastics into valuable carbon-containing products under mild conditions, and traditional wastewater treatment technology cannot efficiently remove microplastics, especially for difficult-to-degradable microplastics such as polyethylene, which are inefficient and costly.

Method used

The lanthanum ferrite catalyst with lanthanum defect is prepared by sol-gel method, and electrons and holes are generated by photocatalytic systems to achieve rapid degradation of microplastics, with a degradation rate of up to 92%, and polyethylene is converted into C7-C16 fat chain carboxylic acids and dicarboxylic acids.

Benefits of technology

It significantly improves the degradation efficiency of microplastics, especially the degradation capacity of polyethylene, realizes efficient and rapid removal of difficult-to-degraded pollutants in actual water environments, and converts microplastics into valuable resource-based products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976503A_ABST
    Figure CN118976503A_ABST
Patent Text Reader

Abstract

The invention discloses a lanthanum ferrite catalyst with lanthanum defects, a preparation method of the lanthanum ferrite catalyst and application of the lanthanum ferrite catalyst in photocatalytic degradation of plastics. The lanthanum ferrite catalyst with the lanthanum defects is LaFeO3 containing La vacancies. The preparation method of the lanthanum-defect lanthanum ferrite catalyst comprises the following steps: mixing lanthanum salt, ferric salt, urea and water, uniformly stirring to obtain a lanthanum ferrite catalyst precursor solution, mixing citric acid and the lanthanum ferrite catalyst precursor solution, uniformly stirring, stirring at 70-80 DEG C until a gel state is obtained to obtain a lanthanum-defect lanthanum ferrite catalyst precursor, and drying to obtain the lanthanum-defect lanthanum ferrite catalyst. And drying and grinding the lanthanum ferrite catalyst precursor with the lanthanum defect, calcining at 750-900 DEG C for 3-5 hours, and cooling to room temperature to obtain the lanthanum ferrite catalyst with the lanthanum defect. The lanthanum ferrite catalyst with lanthanum defects prepared by the invention has relatively strong pollutant degradation and conversion capability on micro-plastics, especially polyethylene. The degradation rate of the PE can reach 92%, and the yield of the product oil which is converted into C7-C16 aliphatic chain carboxylic acid and dicarboxylic acid with lower molecular weight as main components can reach about 70%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of microplastic degradation, and specifically relates to a lanthanum-defective lanthanum ferrite catalyst, a preparation method thereof, and an application thereof in photocatalytic degradation of plastics. Background Art

[0002] Plastics are widely used in various fields of life due to their low cost, strong waterproofness and stable physical and chemical properties. However, due to their stable properties, they cannot be naturally degraded in a short period of time, resulting in the death of many animals in natural habitats due to suffocation caused by accidental ingestion. Plastic products can be decomposed into small-sized plastic particles under physical, chemical and biological conditions. Microplastics (MPs) refer to plastic particles with a diameter of less than 5 mm, accounting for 92.4% of plastic waste, mainly polyethylene (PE), polypropylene (PP), polystyrene (PS), polyvinyl chloride (PVC), polyacrylonitrile (PAN) and polyethylene terephthalate (PET). Compared with plastic pollution, microplastic pollution can lead to more serious environmental, ecological and health problems. Microplastics (MPs) are widely present in the surface layer of aquatic ecosystems, providing a unique ecological niche for the enrichment of microorganisms in the water environment and posing a potential threat to the ecosystem and human health.

[0003] Polyethylene (PE) is highly stable and accounts for the largest proportion of microplastics. The catalytic hydrogenolysis process can effectively convert it into low molecular weight alkane products to re-enter the energy cycle, but the reaction temperature of the catalytic hydrogenolysis process is usually higher than 200 ° C and is highly dependent on H2. At present, H2 mainly comes from fossil fuels, which increases the consumption of fossil fuel energy, promotes carbon dioxide emissions, and further exacerbates the greenhouse effect. Therefore, it is still challenging to develop new processes to convert microplastics into valuable carbon-containing products under mild conditions.

[0004] In domestic research work, Liu Xianrui et al. (Biodegradation and High-Value Conversion of Polyethylene Waste Plastics, Bioprocessing Engineering) reviewed various waste plastic biological treatment technologies, used the supernatant after primary sedimentation, added sufficient reducing agents to reduce microplastics, and analyzed the differences between chemical high-value and biological high-value products of polyethylene waste plastics. They proposed a solution of constructing an artificial system by mixing two or more degradation colonies, but there are still problems such as unclear actual treatment effects and many restrictive factors.

[0005] Traditional wastewater treatment technologies cannot effectively transform and remove microplastics. Advanced oxidation processes (AOPs) have been proven to be effective treatment technologies for drug degradation and mineralization. In recent years, photocatalytic AOPs have received increasing attention in water treatment fields such as the removal of persistent organic pollutants and the decomposition of metal-organic complexes.

[0006] Meng Yachu et al. (CN117843072A) designed a photocatalytic degradation system that can effectively treat microplastics in boiling water. Yuan Haoran et al. (CN117920307A) prepared a nitrogen-deficient oxygen-doped g-C3N4 photocatalyst, which removed 73% of polystyrene, 68% of polypropylene and 64% of polyethylene after 200 hours. However, in the above two patents, the actual removal efficiency of the photocatalyst is still low, requiring long-term treatment and incomplete degradation of pollutants. The actual treatment cost is high and is not suitable for the degradation and transformation of microplastics in actual water bodies. In summary, whether abroad or at home, there is no suitable material that can effectively remove and transform microplastics represented by polyethylene in actual water environments. Summary of the invention

[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide a lanthanum-deficient lanthanum ferrite catalyst.

[0008] Another object of the present invention is to provide a method for preparing the above-mentioned lanthanum-deficient lanthanum ferrite catalyst, which adopts a sol-gel method.

[0009] Another object of the present invention is to provide the use of the above-mentioned lanthanum-deficient lanthanum ferrite catalyst in photocatalytic degradation of plastics. The lanthanum-deficient lanthanum ferrite catalyst generates electrons and holes by light in the photocatalytic system to achieve rapid degradation of different types of microplastics. By manufacturing a perovskite catalyst containing La vacancies in lanthanum ferrite (LaFeO3), after strong alkali pretreatment, the degradation rate (Weight Loss (%)) of PE can reach 92%, and the recovery rate of organic matter converted into C7-C16 fatty chain carboxylic acids and dicarboxylic acids with lower molecular weight can reach about 70%.

[0010] The purpose of the present invention is achieved through the following technical solutions.

[0011] A lanthanum-deficient lanthanum ferrite catalyst is LaFeO3 containing La vacancies.

[0012] A method for preparing a lanthanum-deficient lanthanum ferrite catalyst comprises the following steps:

[0013] S1, mixing lanthanum salt, iron salt, urea and water, stirring until uniform, to obtain a lanthanum ferrite catalyst precursor solution, wherein the ratio of lanthanum in the lanthanum salt, iron in the iron salt and urea is 1:1:(1-6) in terms of molar fractions;

[0014] In S1, the ratio of lanthanum in the lanthanum salt, iron in the iron salt and urea is preferably 1:1:(2-5), more preferably 1:1:3, based on the amount of substances.

[0015] In S1, the ratio of the amount of lanthanum in the lanthanum salt to the volume of water is (0.05-0.2):1, the unit of the amount of lanthanum is mol, and the unit of the volume is mL.

[0016] In S1, the lanthanum salt is lanthanum nitrate hexahydrate, the iron salt is ferric nitrate nonahydrate, and the water is deionized water.

[0017] In S1, the stirring time is at least 20 min, preferably 20 to 40 min.

[0018] S2, mixing citric acid and lanthanum ferrite catalyst precursor solution, stirring until uniform, and then stirring at 70-80° C. until a gel is obtained to obtain a lanthanum-deficient lanthanum ferrite catalyst precursor, wherein the ratio of citric acid to lanthanum in the lanthanum salt is (1-1.2):1 in terms of molar fraction;

[0019] In S2, the stirring time until the mixture is uniform is 1 to 2 hours.

[0020] In S2, the stirring time to a gel state is 3 to 6 hours.

[0021] In S2, the stirring rate to a gel state is 300-700 r / min.

[0022] S3, drying and grinding the lanthanum-deficient lanthanum ferrite catalyst precursor, calcining at 750-900° C. for 3-5 hours, and cooling to room temperature to obtain a lanthanum-deficient lanthanum ferrite catalyst.

[0023] In S3, the drying temperature is 120-150°C, and the drying time is 10-15 hours.

[0024] In S3, the heating rate of the calcination is 5 to 10°C / min.

[0025] In S3, the speed of cooling to room temperature is 5-10°C / min.

[0026] In S3, the gas atmosphere for calcination is air.

[0027] In S3, the room temperature is 20-25°C.

[0028] The use of the above lanthanum-deficient lanthanum ferrite catalyst in photocatalytic degradation of plastics.

[0029] In the above technical solution, the lanthanum-deficient lanthanum ferrite catalyst catalytically degrades plastic under visible light.

[0030] In the above technical solution, the photocatalytic degradation of plastic is carried out at normal temperature and pressure (25° C., 1 standard atmospheric pressure).

[0031] In the above technical solution, the plastic is immersed in a 0.1 mol / L NaOH solution for 24 hours before photocatalytic degradation.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] 1. The preparation method of the present invention is simple and easy to operate.

[0034] 2. The lanthanum-deficient lanthanum ferrite catalyst prepared by the present invention has a strong ability to degrade and transform pollutants to microplastics, especially polyethylene. Compared with the original lanthanum ferrite (LaFeO3) nanomaterial, the lanthanum-deficient lanthanum ferrite catalyst has a nearly 4-fold improvement in the degradation ability of polyethylene, and can achieve the degradation and resource conversion of difficult-to-degrade microplastics represented by polyethylene.

[0035] 3. The lanthanum-deficient lanthanum ferrite catalyst prepared by the present invention can form a mechanism for the coordinated removal of pollutants by electrons and holes, and can achieve efficient and rapid removal of difficult-to-degrade pollutants in actual complex and changeable water environments, and is suitable for use in actual water bodies.

[0036] 4. The lanthanum-deficient lanthanum ferrite catalyst prepared by the present invention has better visible light absorption performance and higher utilization rate compared with the lanthanum ferrite catalyst (LFO). BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 TEM images and element mapping images of the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1, wherein (a) is a TEM image, (b) is a lattice fringe image, (c) is an EDS image of the La element, (d) is an EDS image of the Fe element, and (e) is an EDS image of the O element;

[0038] Figure 2 XRD patterns of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 (the inset is a partial angle magnified view);

[0039] Figure 3(a) specific surface area and (b) pore size distribution of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1;

[0040] Figure 4 The UV-visible diffuse reflectance images of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1;

[0041] Figure 5 The degradation effect diagram of polyethylene by the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1, the lanthanum-deficient lanthanum ferrite catalyst (U-LFO) prepared in Example 2, the lanthanum-deficient lanthanum ferrite catalyst (2U-LFO) prepared in Example 3, the lanthanum-deficient lanthanum ferrite catalyst (6U-LFO) prepared in Example 4, and the lanthanum ferrite catalyst (LFO) prepared in Example 5;

[0042] Figure 6 The degradation effect diagram of different microplastics by the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 and the lanthanum ferrite catalyst (LFO) prepared in Example 5;

[0043] Figure 7 This is a graph showing the degradation effect of the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 on polyethylene in different water environments;

[0044] Figure 8 The figure is a graph showing the degradation effect of the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 on polyethylene under different influencing factors, wherein (a) shows the effect of different pH values ​​on the degradation of polyethylene, (b) shows the effect of different lanthanum-defective lanthanum ferrite catalyst contents on the degradation of polyethylene, (c) shows the effect of different polyethylene concentrations on the degradation effect, and (d) shows the effect of different light stresses on the degradation of polyethylene;

[0045] Fig. 9 (a) is a free radical quenching experimental diagram of the lanthanum ferrite catalyst (LFO) prepared in Example 5, Fig. 9 (b) is a free radical quenching experimental diagram of the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1;

[0046] Fig.10 The electrochemical spectra of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1, wherein (a) is a cyclic voltammogram, (b) is a linear voltammogram, (c) is an electrochemical impedance spectroscopy (EIS) graph, and (d) is an MS graph;

[0047] Fig.11 (a) is a photocurrent transient response diagram of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1, Fig.11 (b) is Fig.11 A partial enlarged view of (a);

[0048] Fig.12 This is the GC-MS graph of the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) after degradation of PE microplastics in Example 1. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0050] The raw materials and their manufacturers' information involved in the following examples are as follows:

[0051] In the following examples, deionized water was used.

[0052] In the following examples, the lanthanum salt is lanthanum nitrate hexahydrate, and the iron salt is iron nitrate nonahydrate.

[0053] Lanthanum nitrate hexahydrate (La(NO3)3·6H2O), ferric nitrate nonahydrate (Fe(NO3)3·9H2O), urea (CO(NH)2) and citric acid were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0054] Citric acid, urea, and metal nitrates (La(NO3)3·6H2O and Fe(NO3)3·9H2O) were of analytical grade.

[0055] The instruments and their model information involved in the following embodiments are as follows:

[0056] A xenon lamp (CEL-HX F300, Beijing, China, 420 nm cutoff filter) was used as the light source (maximum power 350 W).

[0057] The crystallinity of the product was characterized by Rigaku D / Max 2200PC x-ray diffractometer (λ=0.15418 nm).

[0058] The morphology and microstructure were observed by a Talos f200x transmission electron microscope (TEM) equipped with an energy dispersive spectrometer (EDS).

[0059] UV-visible diffuse reflectance spectra (DRS) were recorded on a UV-3600i Plus UV-visible spectrophotometer (Shimadzu).

[0060] N2 adsorption-desorption isotherms were recorded using an automatic gas adsorption analyzer (Quantachrome).

[0061] The content of microplastics was determined by weighing method, and GC-MS was used to quantitatively analyze microplastics and their transformation products.

[0062] The photoelectrochemical experiments were carried out on an electrochemical workstation (Shanghai Chenhua CHI660B).

[0063] Embodiments 1 to 4

[0064] A method for preparing a lanthanum-deficient lanthanum ferrite catalyst comprises the following steps:

[0065] S1, lanthanum salt (La(NO3)3·6H2O), iron salt (Fe(NO3)3·9H2O), urea (CO(NH)2) and water are mixed, and magnetically stirred at 500 r / min for 20 min until uniform, to obtain a lanthanum ferrite catalyst precursor solution, wherein, in terms of molar fractions, the ratio of lanthanum in the lanthanum salt, iron in the iron salt and urea is W, the ratio of the molar fraction of lanthanum in the lanthanum salt to the volume fraction of water is 0.1:1, the unit of the molar fraction is mol, and the unit of the volume fraction is mL;

[0066] S2, mixing citric acid and lanthanum ferrite catalyst precursor solution, stirring for 1 hour until uniform, and then magnetically stirring at 500 r / min in a 70° C. water bath for 3 hours until water evaporates to form a gel, to obtain a lanthanum-deficient lanthanum ferrite catalyst precursor, wherein the ratio of citric acid to lanthanum in the lanthanum salt in S1 is 1.05:1 in terms of molar fraction;

[0067] S3, drying the lanthanum-deficient lanthanum ferrite catalyst precursor at 120°C for 12h, taking it out, grinding it in a mortar, putting it into a crucible in a muffle furnace, raising the temperature to 800°C at a heating rate of 5°C / min in an air atmosphere and calcining it at 800°C for 3h, and then cooling the temperature to room temperature (20-25°C) at a heating rate of 5°C / min after calcination to obtain a lanthanum-deficient lanthanum ferrite catalyst.

[0068] The W and serial numbers of the lanthanum-deficient lanthanum ferrite catalysts prepared in Examples 1 to 4 are shown in Table 1.

[0069] Table 1

[0070] Example W Numbering of lanthanum-defective lanthanum ferrite catalysts Example 1 1:1:3 3U-LFO Example 2 1:1:1 U-LFO Example 3 1:1:2 2U-LFO Example 4 1:1:6 6U-LFO

[0071] Example 5

[0072] A lanthanum ferrite catalyst (LFO) is prepared by a method substantially identical to that of the above-mentioned Example 1, the only difference being that urea (CO(NH)2) is not added in this Example.

[0073] Figure 1 TEM image of the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 and the element mapping image of the lanthanum-deficient lanthanum ferrite catalyst. Figure 1 As shown in (a), the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 was successfully synthesized, and the crystals were in the form of flakes. Figure 1 (b) shows that the lattice fringe spacing of the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 is 0.283 nm, which is slightly smaller than the lanthanum ferrite spacing (the lattice fringe spacing of the lanthanum ferrite catalyst (LFO) prepared in Example 5 is 0.285 nm), indicating that the lanthanum-deficient lanthanum ferrite catalyst constructed in Example 1 achieves the absence of La atoms. Figure 1 (c) is the EDS image of the La element of the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1, which further verifies the generation of La defects. Figure 1 As can be seen from (c), (d) and (e), the different elements are evenly distributed inside the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1.

[0074] Figure 2 The XRD patterns of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 are shown in Table 1. Figure 2 It can be seen that after the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 constructs the La defect, the diffraction peak shifts toward the high angle direction. The reason is that the appearance of the La defect causes the A site vacancy in the perovskite, thereby exposing more Fe sites, which causes the diffraction peak to shift toward the high angle direction, verifying the appearance of the La defect.

[0075] Figure 3 The (a) specific surface area and (b) pore size distribution diagram of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 are shown in FIG. Figure 3 As shown in (a), the specific surface area (10.69 m -2 g -1 ) is larger than the specific surface area (8.09 m -2 g -1 ),Depend on Figure 3 As can be seen from (b), the pore size of 3U-LFO is smaller than that of LFO, and the preparation is more uniform, verifying its better specific surface area.

[0076] Figure 4The UV-visible diffuse reflectance images of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 are shown in FIG. Figure 4 It can be seen that the lanthanum-defective lanthanum ferrite catalyst prepared in Example 1 has a higher response not only in the visible light region, but also in the near-infrared light region, indicating that the lanthanum-defective lanthanum ferrite catalyst can achieve effective utilization of visible light and near-infrared light.

[0077] Method for degrading microplastic pollutants by catalyst under visible light: soak the microplastics in 1 mol / L sodium hydroxide aqueous solution for 24 hours, filter, rinse with water and ethanol several times and take out, dry in an oven at 80°C for 12 hours, and obtain microplastics treated with strong alkali, wherein the microplastics are one of polyethylene (PE), polypropylene (PP), polyvinyl chloride (PVC) and polyacrylonitrile (PAN). Microplastics with a mass of m0 (m0 is 100 mg) treated with strong alkali are uniformly dispersed in water to prepare a microplastic aqueous solution with a microplastic concentration of 1 g / L, and the pH of the microplastic aqueous solution is ≈ 7 (slightly higher than 7), wherein the water is one of deionized water, tap water, lake water and secondary sewage.

[0078] 25 mg of catalyst was added to 100 mL of microplastic aqueous solution (i.e., microplastics with a mass m0 of 100 mg were uniformly dispersed in 100 mL of water), and the degradation of microplastics was carried out at a speed of 500 r / min under irradiation of a 25W xenon lamp (with a filter added to make the wavelength greater than 420 nm). The degradation time was 12 h, and the obtained sample was filtered to remove the catalyst and water, and then dried and weighed. The mass was recorded as m. After the experiment, the xenon lamp was turned off to terminate the reaction. Among them, the catalyst is one of the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1, the lanthanum-defective lanthanum ferrite catalyst (U-LFO) prepared in Example 2, the lanthanum-defective lanthanum ferrite catalyst (2U-LFO) prepared in Example 3, the lanthanum-defective lanthanum ferrite catalyst (6U-LFO) prepared in Example 4, and the lanthanum ferrite catalyst (LFO) prepared in Example 5.

[0079] Calculation method of Weight Loss (%): WL = m0-m / m0.

[0080] According to the “method for degrading microplastic pollutants under visible light using a catalyst”, one of the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1, the lanthanum-deficient lanthanum ferrite catalyst (U-LFO) prepared in Example 2, the lanthanum-deficient lanthanum ferrite catalyst (2U-LFO) prepared in Example 3, the lanthanum-deficient lanthanum ferrite catalyst (6U-LFO) prepared in Example 4, and the lanthanum ferrite catalyst (LFO) prepared in Example 5 was used as a catalyst to degrade PE (microplastics are polyethylene (PE)) (water is deionized water), and the Weight Loss (%) when the degradation time is 12h is as follows: Figure 5 As shown, it can be seen that the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 has the highest degradation effect on polyethylene and can degrade 92% of polyethylene in 12 hours.

[0081] According to the “Method for Degrading Microplastic Pollutants with Catalysts under Visible Light”, one of the lanthanum-deficient lanthanum ferrite (3U-LFO) prepared in Example 1 and the lanthanum ferrite catalyst (LFO) prepared in Example 5 was used as a catalyst to degrade one of PE, PP, PVC and PAN (the water was deionized water), and the degradation effect of the catalyst on other microplastic pollutants was tested. The Weight Loss (%) when the degradation time was 12 h was as follows: Figure 6 As shown, compared with the lanthanum ferrite catalyst (LFO) prepared in Example 5, the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 can achieve efficient degradation of microplastic pollutants within 12 hours.

[0082] According to the “Method for Degrading Microplastic Pollutants by Catalysts under Visible Light”, the lanthanum-deficient lanthanum ferrite (3U-LFO) prepared in Example 1 was used as a catalyst for degradation (the microplastics were polyethylene (PE), and the water was one of deionized water, tap water, lake water and secondary sewage). The Weight Loss (%) when the degradation time was 12 h was as follows: Figure 7 As shown, it can be seen that the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 can still degrade at least 80% of polyethylene in 12 hours under different water quality conditions.

[0083] Experiment on degradation of polyethylene under different influencing factors: After polyethylene is placed in a 1mol / L sodium hydroxide aqueous solution and soaked for 24 hours, it is filtered, rinsed with water and ethanol several times and taken out, and dried in an oven at 80°C for 12 hours to obtain polyethylene treated with strong alkali. The polyethylene treated with strong alkali with a mass of m1 is uniformly dispersed in 100mL deionized water to prepare a polyethylene aqueous solution, and the pH of the polyethylene aqueous solution is adjusted to p by dripping hydrochloric acid (0.1mol / L) or sodium hydroxide aqueous solution (0.1mol / L). The lanthanum-deficient lanthanum iron oxide catalyst prepared in Example 1 with a mass of m3 is added to 100mL of polyethylene aqueous solution, and the polyethylene is degraded for 12 hours under the irradiation of a xenon lamp (adding a filter to make the wavelength greater than 420nm) at a speed of 500r / min. After removing the lanthanum-deficient lanthanum iron oxide catalyst and water from the obtained sample, it is filtered, dried and weighed, and the mass is recorded as m2. After the experiment, the xenon lamp is turned off to end the reaction.

[0084] In the "degradation of polyethylene under different influencing factors" experiment, when m3 = 25 mg, the xenon lamp illumination intensity is 25 W, and m1 is 100 mg, p is adjusted to 3, 5, 7, 9 or 11, the Weight Loss of polyethylene is as follows: Figure 8 As shown in (a). Figure 8 It can be seen from (a) that the lanthanum-deficient lanthanum ferrite catalyst prepared in Example 1 has the best degradation effect on polyethylene (PE) under neutral conditions.

[0085] In the "degradation of polyethylene under different influencing factors" experiment, when p = 7, the xenon lamp illumination intensity is 25W, and m1 is 100mg, adjust m3 = 5mg, 10mg, 15mg, 20mg or 25m, the Weight Loss of polyethylene is as follows Figure 8 As shown in (b). Figure 8 As can be seen from (b), as the content of the lanthanum-deficient lanthanum ferrite catalyst prepared in Example 1 increases, its degradation effect on PE continues to improve.

[0086] In the "degradation of polyethylene under different influencing factors" experiment, when m3 = 25 mg, the xenon lamp illumination intensity is 25 W, and p = 7, m1 is adjusted to 50 mg, 100 mg, 150 mg, 200 mg, or 250 mg. The Weight Loss of polyethylene is as follows: Figure 8 as shown in (c).

[0087] In the "degradation of polyethylene under different influencing factors" experiment, when m3 = 25 mg, m1 is 100 mg, p = 7, the xenon lamp illumination intensity is adjusted to 5W, 10W, 15W, 20W or 25W, the Weight Loss of polyethylene is as follows: Figure 8 As shown in (d), from Figure 8It can be seen from (d) that the best degradation effect can be achieved under a light intensity of 25W.

[0088] Figure 8 The calculation method of Weight Loss (%) is: WL = m1-m2 / m1.

[0089] Fig. 9 (a) is a free radical quenching experiment diagram of the lanthanum ferrite catalyst (LFO) prepared in Example 5 after degradation for 12 hours. Fig. 9 (b) Radical quenching experiment diagram of the degradation of lanthanum-defective lanthanum ferrite catalyst (3U-LFO) in Example 1 for 12 hours. According to the “Method for Degrading Microplastic Pollutants by Catalysts under Visible Light”, the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 and the lanthanum ferrite catalyst (LFO) prepared in Example 5 were used as catalysts to degrade PE (water was deionized water), and the experimental results were respectively taken as “Blank” in Figures (a) and (b), referring to the “Blank” experimental method. Five groups of quenching experiments were set up for each catalyst. 10mmol of quencher was added before deuterium lamp irradiation. The quencher was one of tert-butyl alcohol (TBA), carotene, potassium dichromate (K2Cr2O7), disodium ethylenediaminetetraacetate (EDTA-2Na) and superoxide dismutase (SOD). Tert-butyl alcohol quenched the hydroxyl radical OH in the system, carotene quenched the singlet oxygen in the system, potassium dichromate quenched the electron in the system, and EDTA-2Na quenched the hole h in the system. + and SOD to quench superoxide free radicals·O2 - To determine the types of species that play a major role in the degradation of microplastics. Fig. 9 As shown in the figure, the degradation system of polyethylene by lanthanum-defective lanthanum ferrite catalyst is a photocatalytic system, and the main role in the degradation process is played by the hole h + , achieving efficient separation and utilization of electrons and holes, and electrons are also converted into superoxide radicals·O2 through reactions, so efficient degradation of microplastics can be achieved. At the same time, efficient degradation of microplastics can also be achieved in actual complex water bodies.

[0090] Fig.10 These are the electrochemical property test graphs of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) in Example 1, wherein (a) is a cyclic voltammogram, (b) is a linear voltammogram, (c) is an electrochemical impedance spectroscopy (EIS) graph, and (d) is a Mott-Schottky curve graph (MS graph). Fig.10 (a) and (b) show that the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) in Example 1 has more electron mobility and produces more electrons. Fig.10(c) and (d) show that the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) in Example 1 has smaller impedance, higher conductivity and carrier concentration than the lanthanum ferrite catalyst (LFO) prepared in Example 5, confirming that lanthanum defects do accelerate the photoexcited carrier transfer kinetics.

[0091] Fig.11 (a) is a photocurrent transient response diagram of the lanthanum ferrite catalyst (LFO) prepared in Example 5 and the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1, Fig.11 (b) is Fig.11 Partially enlarged view of (a). The results show that the instantaneous photoelectron concentration of the lanthanum-defective lanthanum ferrite catalyst (3U-LFO) prepared in Example 1 is higher than that of the lanthanum ferrite catalyst (LFO) prepared in Example 5, and its photoelectron self-annihilation rate is lower than that of the lanthanum ferrite catalyst (LFO) prepared in Example 5. The above photophysical research clearly proves that the structure of La defects realizes the effective separation of electrons and holes, slows down the rate of their self-annihilation, and thus realizes the improvement of photocatalytic activity.

[0092] Fig.12 This is the GC-MS graph of the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) after degradation of PE microplastics in Example 1. The appearance of each peak indicates the appearance of different carbon chain substances. According to the determination method of different substances, the peaks that appear with the extension of the vertical coordinate peak time correspond to hydrocarbon chain substances containing different numbers of carbon atoms, and the relative height and area of ​​the peaks correspond to the relative content of hydrocarbon chain substances. The GC-MS results show that the peak with a peak time of 1.33min corresponds to methane, the peak with a peak time of 18.92min corresponds to the fatty hydrocarbon chain of C8, the peak with a peak time of 21.96min corresponds to the fatty hydrocarbon chain of C10, and the peak with a peak time of 25.74min corresponds to the fatty hydrocarbon chain of C12. The sharp small peaks that appear during this period indicate the appearance of different derivatives with the same number of C atoms. According to the standard spectrum of GC-MS, the main products generated after the degradation of PE microplastics by the lanthanum-deficient lanthanum ferrite catalyst (3U-LFO) in Example 1 are fatty chain carboxylic acids and dicarboxylic acids of C7-C16, indicating that the system successfully selectively oxidizes PE into long-chain organic matter, achieving the goal of resource utilization of microplastics. According to the integral calculation of the peak area, about 70wt% of PE is degraded to generate C7-C16 long-chain aliphatic carboxylic acids and dicarboxylic acids. Long-chain aliphatic carboxylic acids and dicarboxylic acids are raw materials for synthesizing high-grade fragrances and high-performance nylons, and have objective utilization value, realizing the resource upgrading of PE microplastics. The recycling experiment proves the stability and application prospects of the catalyst.

[0093] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A lanthanum-deficient lanthanum ferrite catalyst, It is characterized in that It is LaFeO containing La vacancies 3 .

2. A method for preparing a lanthanum-deficient lanthanum ferrite catalyst, It is characterized in that The following steps are involved: S1, mixing lanthanum salt, iron salt, urea and water, stirring until uniform, to obtain a lanthanum ferrite catalyst precursor solution, wherein the ratio of lanthanum in the lanthanum salt, iron in the iron salt and urea is 1:1:(1-6) in terms of molar fractions; S2, mixing citric acid and lanthanum ferrite catalyst precursor solution, stirring until uniform, and then stirring at 70-80° C. until a gel is obtained to obtain a lanthanum-deficient lanthanum ferrite catalyst precursor, wherein the ratio of citric acid to lanthanum in the lanthanum salt is (1-1.2):1 in terms of molar fraction; S3, drying and grinding the lanthanum-deficient lanthanum ferrite catalyst precursor, calcining at 750-900° C. for 3-5 hours, and cooling to room temperature to obtain a lanthanum-deficient lanthanum ferrite catalyst.

3. The preparation method according to claim 2, It is characterized in that In S1, the ratio of lanthanum in the lanthanum salt, iron in the iron salt and urea is preferably 1:1:(2-5), more preferably 1:1:3, calculated by molar fraction.

4. The preparation method according to claim 2, It is characterized in that In S1, the ratio of the amount of lanthanum in the lanthanum salt to the volume of water is (0.05-0.2):1, the unit of the amount of lanthanum is mol, and the unit of the volume is mL.

5. The preparation method according to claim 2, It is characterized in that In S1, the stirring time is at least 20 minutes.

6. The preparation method according to claim 2, It is characterized in that In S2, the stirring time until the mixture is in a gel state is 3 to 6 hours.

7. The preparation method according to claim 2, It is characterized in that In S3, the gas atmosphere for calcination is air.

8. The preparation method according to claim 2, It is characterized in that In S3, the heating rate of the calcination is 5 to 10°C / min.

9. Use of the lanthanum-deficient lanthanum ferrite catalyst as claimed in claim 1 in photocatalytic degradation of plastics.

10. Use of the lanthanum-deficient lanthanum ferrite catalyst obtained by the preparation method as claimed in claim 2 in photocatalytic degradation of plastics.

Citation Information

Patent Citations

  • Photocatalytic degradation system

    CN117843072A

  • Preparation of nitrogen-deficient oxygen-doped graphite-phase carbon nitride photocatalyst and application of nitrogen-deficient oxygen-doped graphite-phase carbon nitride photocatalyst in micro-plastic treatment in water

    CN117920307A

  • Method for preparing nanometer lanthanum ferrite powder by using microwave process

    CN102408132A

  • Preparation method for titanium dioxide nanotube array modified by lanthanum ferrite nanoparticles

    CN106702462A

  • Method for catalytically degrading antibiotic wastewater by double perovskite La2NiFeO6

    CN111545212A