Application of Ni / SrO-Sm2O3 catalyst in hydrogen production through thermocatalytic ammonia decomposition

By preparing Ni/SrO-Sm2O3 catalyst, the support effect of SrO and Sm2O3 was used to solve the problem of high-temperature hydrogen poisoning, promote ammonia decomposition and hydrogen production, improve the stability and activity of the catalyst, and achieve efficient ammonia decomposition and hydrogen production reaction.

CN118976505AActive Publication Date: 2024-11-19HUNAN UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411463764.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-19
Estimated Expiration
2044-10-21

AI Technical Summary

Technical Problem

Under high temperature and H2 atmospheres, active metals are prone to hydrogen poisoning to form stable M-H bonds, resulting in catalyst deactivation. The prior art is difficult to promote N-H dissociation and N2 desorption at the same time, affecting the efficiency of ammonia decomposition and hydrogen production.

Method used

The Ni/SrO-Sm2O3 catalyst was prepared by co-precipitation hydrothermal method and high-temperature pyrolysis treatment. SrO was used as an alkaline support to improve the electron state of Ni, and the hydroxyl group on the surface of Sm2O3 promoted hydrogen overflow. Prevent catalyst hydrogen poisoning, form new intermediate product SmOH2, and improve catalytic activity.

Benefits of technology

The stable structure and high activity of the catalyst are achieved, hydrogen poisoning is prevented, the efficiency of thermally catalyzed ammonia decomposition is improved, and the thermal catalytic activity and conversion frequency (TOF value) of the catalyst is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976505A_ABST
    Figure CN118976505A_ABST
Patent Text Reader

Abstract

The invention discloses an application of a Ni / SrO-Sm2O3 catalyst in hydrogen production through thermocatalytic ammonia decomposition, which comprises the following steps: dispersing soluble Ni salt, Sr salt and Sm salt in water, uniformly mixing, and carrying out coprecipitation and hydrothermal treatment to obtain a composite hydroxide; performing high-temperature pyrolysis on the composite hydroxide to obtain a composite oxide nanorod; and finally, carrying out high-temperature hydrogen treatment on the composite oxide nanorod to obtain the nanorod-shaped Ni / SrO-Sm2O3 catalyst. The catalyst has a stable structure, Ni in the catalyst is uniformly dispersed, Ni is used as an active site in a thermocatalytic reaction, SrO is used as an alkaline carrier to improve the electronic state of Ni, Sm2O3 is used as a hydrogen overflow carrier to relieve hydrogen poisoning, a surface hydroxyl group promotes generation of a new intermediate product (SmOH2), and the catalyst has excellent thermocatalytic activity in thermocatalytic ammonia decomposition hydrogen production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen production by decomposition of ammonia, and specifically relates to application of a Ni / SrO-Sm2O3 catalyst in hydrogen production by thermal catalytic decomposition of ammonia. Background Art

[0002] The decomposition kinetics of NH3 on metals (denoted as M) depends on the strength of the MN bond. A stronger MN bond is conducive to the dissociation of NH in the NH3 molecule, but is not conducive to the desorption of N2 products on the catalyst surface; on the contrary, a weaker MN bond is conducive to the desorption of N2, but hinders the dissociation of the NH bond. Moderate MN bond strength, which is easy for NH dissociation and N2 desorption, is crucial to promote the decomposition of ammonia. Most of the current work is mainly aimed at solving the problem of MN bond strength. However, under high temperature and H2 atmosphere, active metals are easily poisoned by hydrogen to form stable MH bonds, resulting in catalyst deactivation. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide an application of a Ni / SrO-Sm2O3 catalyst in thermal catalytic ammonia decomposition to produce hydrogen. The catalyst has a stable structure and Ni is uniformly dispersed in the catalyst. Ni serves as an active site in the thermal catalytic reaction, SrO serves as an alkaline carrier to improve the electronic state of Ni, and Sm2O3 serves as a hydrogen overflow carrier to alleviate hydrogen poisoning. The hydroxyl groups on its surface promote the formation of a new intermediate product (SmOH2), and the catalyst has excellent thermal catalytic activity in thermal catalytic ammonia decomposition to produce hydrogen.

[0004] In order to achieve the above technical objectives, the present invention adopts the following technical solutions: The invention discloses an application of a Ni / SrO-Sm2O3 catalyst in the production of hydrogen by thermal catalytic decomposition of ammonia. The preparation process of the Ni / SrO-Sm2O3 catalyst is as follows: firstly, soluble Ni salt, Sr salt and Sm salt are dispersed in water and uniformly mixed, and composite hydroxide is obtained by coprecipitation and hydrothermal treatment; then, the composite hydroxide is pyrolyzed at high temperature to obtain composite oxide nanorods; finally, the composite oxide nanorods are treated with high temperature hydrogen to obtain nanorod-shaped Ni / SrO-Sm2O3 catalyst; and then the catalyst is used for the production of hydrogen by thermal catalytic decomposition of ammonia.

[0005] Preferably, the soluble Ni salt, Sr salt and Sm salt are all nitrates of each other, and the molar ratio of the soluble Ni salt, the soluble Sr salt and the soluble Sm salt is 1:0.5-0.8:0.2-0.5.

[0006] Preferably, the alkali used in the coprecipitation process is one of sodium hydroxide, potassium hydroxide and ammonia water.

[0007] Preferably, the temperature of the hydrothermal treatment is 160-200°C and the time is 5-15h.

[0008] Preferably, the high temperature pyrolysis temperature is 600-700°C and the time is 4-6h.

[0009] Preferably, the atmosphere of the high temperature hydrogen treatment is a 6% H2 / Ar mixed atmosphere, the temperature is 550-650°C, and the time is 3-5h.

[0010] Advantages of the present invention: The present invention realizes the loading of metal Ni on mixed oxide SrO-Sm2O3 through a co-precipitation hydrothermal method and high-temperature pyrolysis treatment in a reducing atmosphere to obtain Ni / SrO-Sm2O3. The composite material is a nanorod-like structure with uniform active centers and highly exposed active sites. SrO serves as an alkaline carrier to improve the electronic state of Ni. A large number of hydroxyl groups on the surface of Sm2O3 can serve as H overflow binding sites, promoting the transfer of hydrogen from active metal Ni to the surface hydroxyl groups of the Sm2O3 carrier, promoting the generation of a new intermediate product (SmOH2), effectively preventing hydrogen poisoning of the catalyst, and improving the TOF value of the catalyst. The obtained Ni / SrO-Sm2O3 has excellent thermal catalytic activity in thermal catalytic ammonia decomposition to produce hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 The Ni / Sr prepared in Example 1 0.6 Sm 0.4 O x SEM images of like Figure 1 As shown, Ni / Sr 0.6 Sm 0.4 O x The microscopic morphology is nanorod-like.

[0012] Figure 2 The XRD patterns of the catalysts prepared in Examples 1-3 and Comparative Examples 1-2; like Figure 2 As shown, since SrO easily reacts with CO2 in the air, the composite catalyst is composed of SrCO3, Sm2O3 and Ni.

[0013] Figure 3 This is the high temperature XRD pattern of Ni / SrO prepared in Comparative Example 2; like Figure 3 As shown, under the reaction conditions, Sr exists in the form of SrO, which indirectly indicates the successful preparation of the catalyst.

[0014] Figure 4 The Ni / Sr prepared in Example 1 0.6 Sm 0.4 Ox XPS spectrum of like Figure 4 As shown, the hydroxyl content on the catalyst surface is 59.61%, which contains a large amount of hydroxyl groups.

[0015] Figure 5 FTIR graphs of the catalysts prepared in Example 1 and Comparative Examples 1-2; like Figure 5 As shown, the surfaces of the samples of Example 1 and Comparative Example 1 have hydroxyl groups, while the surface of the sample of Comparative Example 1 indicates that the hydroxyl groups on the surface of the material are mainly contributed by Sm2O3.

[0016] Figure 6 The Ni / Sr prepared in Example 1 0.6 Sm 0.4 O x In Situ FTIR spectrum; like Figure 6 As shown, with the introduction of hydrogen, SmOH2 and hydroxyl species are gradually formed on the sample surface, indicating the generation of a new intermediate species SmOH2.

[0017] Figure 7 Ni / Sr prepared in Comparative Example 3 0.6 Sm 0.4 O x - XRD spectrum of bulk; like Figure 7 As shown, the same as Example 1-3, is composed of SrCO3, Sm2O3 and Ni.

[0018] Figure 8 Ni / Sr prepared in Comparative Example 3 0.6 Sm 0.4 O x - SEM spectrum of the block; like Figure 8 As shown, the microstructure of Comparative Example 3 is irregular blocks. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below with reference to the embodiments, but the protection scope of the present invention is not limited to these embodiments.

[0020] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0021] Thermal catalytic ammonia decomposition to produce hydrogen: Weigh 20 mg of catalyst and add it into a quartz reaction tube. Pass pure ammonia (99.999%) in the range of 400°C-600°C with a temperature gradient of 50°C. Test each temperature point for 40 minutes and detect the ammonia conversion rate by gas chromatography.

[0022] Example 1

[0023] Ni / Sr 0.6 Sm 0.4 O x : (1) Dissolve 2mmolNi(NO3)2·6H2O, 1.2mmolSr(NO3)2, and 0.8mmolSm(NO3)3·6H2O in 360mLH2O, stir to dissolve, and then add 40mL1mol·L -1 KOH, after standing for 10 min, remove 320 mL of supernatant, transfer the remaining 80 mL of liquid and precipitate to a 100 mL hydrothermal autoclave, react at 180 °C for 10 h, cool and centrifuge, wash with water 3 times, and dry.

[0024] (2) The obtained precursor powder was heated in a muffle furnace at 5 °C min -1 The heating rate was increased to 650°C and then cooled to room temperature after keeping the temperature for 5 h.

[0025] (3) Then, the mixture was heated in a tube furnace (atmosphere of 6% H2 / Ar) at 5°C min -1 The heating rate was increased to 600°C and kept for 4 hours, and then the target catalyst was obtained after cooling to room temperature.

[0026] The prepared Ni / Sr 0.6 Sm 0.4 O x The catalyst is used for the thermal catalytic decomposition of ammonia to produce hydrogen. Under the conditions of 550°C and pure NH3 (99.999%), the hydrogen production rate of the catalyst is 30.74mmolg (cat) -1 ·min -1 .

[0027] Example 2

[0028] Ni / Sr 0.5 Sm 0.5 O x : (1) Dissolve 2mmolNi(NO3)2·6H2O, 1mmolSr(NO3)2, and 1mmolSm(NO3)3·6H2O in 360mLH2O, stir to dissolve, and then add 40mL1mol·L -1KOH, after standing for 10 min, remove 320 mL of supernatant, transfer the remaining 80 mL of liquid and precipitate to a 100 mL hydrothermal autoclave, react at 180 °C for 10 h, cool and centrifuge, wash with water 3 times, and dry.

[0029] (2) The obtained precursor powder was heated in a muffle furnace at 5 °C min -1 The heating rate was increased to 650°C and then cooled to room temperature after keeping the temperature for 5 h.

[0030] (3) Then, the mixture was heated in a tube furnace (atmosphere of 6% H2 / Ar) at 5°C min -1 The heating rate was increased to 600°C and kept for 4 hours, and then the target catalyst was obtained after cooling to room temperature.

[0031] The prepared Ni / Sr 0.5 Sm 0.5 O x The catalyst is used for the thermal catalytic decomposition of ammonia to produce hydrogen. Under the conditions of 550°C and pure NH3 (99.999%), the hydrogen production rate of the catalyst is 29.39mmolg (cat) -1 ·min -1 .

[0032] Example 3

[0033] Ni / Sr 0.8 Sm 0.2 O x : (1) Dissolve 2mmolNi(NO3)2·6H2O, 1.6mmolSr(NO3)2, and 0.4mmolSm(NO3)3·6H2O in 360mLH2O, stir to dissolve, and then add 40mL1mol·L -1 KOH, after standing for 10 min, remove 320 mL of supernatant, transfer the remaining 80 mL of liquid and precipitate to a 100 mL hydrothermal autoclave, react at 180 °C for 10 h, cool and centrifuge, wash with water 3 times, and dry.

[0034] (2) The obtained precursor powder was heated in a muffle furnace at 5 °C min -1 The heating rate was increased to 650°C and then cooled to room temperature after keeping the temperature for 5 h.

[0035] (3) Then, the mixture was heated in a tube furnace (atmosphere of 6% H2 / Ar) at 5°C min -1 The heating rate was increased to 600°C and kept for 4 hours, and then the target catalyst was obtained after cooling to room temperature.

[0036] The prepared Ni / Sr 0.8 Sm 0.2 O xThe catalyst is used for the thermal catalytic decomposition of ammonia to produce hydrogen. Under the conditions of 550°C and pure NH3 (99.999%), the hydrogen production rate of the catalyst is 29.86mmolg (cat) -1 ·min -1 .

[0037] Comparative Example 1 Ni / Sm2O3: (1) Dissolve 2mmolNi(NO3)2·6H2O and 2mmolSm(NO3)3·6H2O in 360mLH2O, stir to dissolve, and then add 40mL1mol·L -1 KOH, after standing for 10 min, remove 320 mL of supernatant, transfer the remaining 80 mL of liquid and precipitate to a 100 mL hydrothermal autoclave, react at 180 °C for 10 h, cool and centrifuge, wash with water 3 times, and dry.

[0038] (2) The obtained precursor powder was heated in a muffle furnace at 5 °C min -1 The heating rate was increased to 650°C and then cooled to room temperature after keeping the temperature for 5 h.

[0039] (3) Then, the mixture was heated in a tube furnace (atmosphere of 6% H2 / Ar) at 5°C min -1 The heating rate was increased to 600°C and kept for 4 hours, and then the target catalyst was obtained after cooling to room temperature.

[0040] The prepared Ni / Sm2O3 catalyst was used for the thermal catalytic decomposition of ammonia to produce hydrogen. Under the conditions of 550℃ and pure NH3 (99.999%), the hydrogen production rate of the catalyst was 11.02mmolg (cat) -1 ·min -1 .

[0041] Comparative Example 2 Ni / SrO: (1) Dissolve 2mmolNi(NO3)2·6H2O and 2mmolSr(NO3)2 in 360mLH2O, stir to dissolve, and then add 40mL1mol·L -1 KOH, after standing for 10 min, remove 320 mL of supernatant, transfer the remaining 80 mL of liquid and precipitate to a 100 mL hydrothermal autoclave, react at 180 °C for 10 h, cool and centrifuge, wash with water 3 times, and dry.

[0042] (2) The obtained precursor powder was heated in a muffle furnace at 5 °C min -1 The heating rate was increased to 650°C and then cooled to room temperature after keeping the temperature for 5 h.

[0043] (3) Then, the mixture was heated in a tube furnace (atmosphere of 6% H2 / Ar) at 5°C min -1 The heating rate was increased to 600°C and kept for 4 hours, and then the target catalyst was obtained after cooling to room temperature.

[0044] The prepared Ni / SrO catalyst was used for the thermal catalytic decomposition of ammonia to produce hydrogen. Under the conditions of 550°C and pure NH3 (99.999%), the hydrogen production rate of the catalyst was 8.18 mmol / g (cat) -1 ·min -1 .

[0045] Comparative Example 3 Ni / Sr 0.6 Sm 0.4 O x - Blocky: (1) Add 2 mmol Ni(NO3)2·6H2O, 1.2 mmol Sr(NO3)2, 0.8 mmol Sm(NO3)3·6H2O, and 4.8 mmol citric acid to 80 mL water and stir vigorously in an 80 °C water bath until the water evaporates. The resulting precursor is dried at 100 °C overnight.

[0046] (2) The obtained precursor powder was heated in a muffle furnace at 5 °C min -1 The heating rate was increased to 600°C and kept at this temperature for 5 h before being lowered to room temperature.

[0047] (3) Then, the mixture was heated in a tube furnace (atmosphere of 6% H2 / Ar) at 5°C min -1 The heating rate was increased to 600°C and kept for 4 hours, and then the target catalyst was obtained after cooling to room temperature.

[0048] The prepared Ni / SrO catalyst was used for the thermal catalytic decomposition of ammonia to produce hydrogen. Under the conditions of 550°C and pure NH3 (99.999%), the hydrogen production rate of the catalyst was 17.70 mmol / g (cat) -1 ·min -1 .

[0049] Comparative Example 4 Ni / Mg 0.6 Sm 0.4 O x : (1) Dissolve 2mmolNi(NO3)2·6H2O, 1.2mmolMg(NO3)2, and 0.8mmolSm(NO3)3·6H2O in 360mLH2O, stir to dissolve, and then add 40mL1mol·L -1KOH, after standing for 10 min, remove 320 mL of supernatant, transfer the remaining 80 mL of liquid and precipitate to a 100 mL hydrothermal autoclave, react at 180 °C for 10 h, cool and centrifuge, wash with water 3 times, and dry.

[0050] (2) The obtained precursor powder was heated in a muffle furnace at 5 °C min -1 The heating rate was increased to 650°C and then cooled to room temperature after keeping the temperature for 5 h.

[0051] (3) Then, the mixture was heated in a tube furnace (atmosphere of 6% H2 / Ar) at 5°C min -1 The heating rate was increased to 600°C and kept for 4 hours, and then the target catalyst was obtained after cooling to room temperature.

[0052] The prepared Ni / Mg 0.6 Sm 0.4 O x The catalyst is used for the thermal catalytic decomposition of ammonia to produce hydrogen. Under the conditions of 550°C and pure NH3 (99.999%), the hydrogen production rate of the catalyst is 21.38mmolg (cat) -1 ·min -1 .

[0053] Comparative Example 5 Ni / Sr 0.6 Y 0.4 O x : (1) Dissolve 2mmolNi(NO3)2·6H2O, 1.2mmolSr(NO3)2, and 0.8mmolY(NO3)3·6H2O in 360mLH2O, stir to dissolve, and then add 40mL1mol·L -1 KOH, after standing for 10 min, remove 320 mL of supernatant, transfer the remaining 80 mL of liquid and precipitate to a 100 mL hydrothermal autoclave, react at 180 °C for 10 h, cool and centrifuge, wash with water 3 times, and dry.

[0054] (2) The obtained precursor powder was heated in a muffle furnace at 5 °C min -1 The heating rate was increased to 650°C and then cooled to room temperature after keeping the temperature for 5 h.

[0055] (3) Then, the mixture was heated in a tube furnace (atmosphere of 6% H2 / Ar) at 5°C min -1 The heating rate was increased to 600°C and kept for 4 hours, and then the target catalyst was obtained after cooling to room temperature.

[0056] The prepared Ni / Sr 0.6 Y 0.4 O xThe catalyst is used for the thermal catalytic decomposition of ammonia to produce hydrogen. Under the conditions of 550°C and pure NH3 (99.999%), the hydrogen production rate of the catalyst is 25.05mmolg (cat) -1 ·min -1 .

Claims

1. Application of Ni / SrO-Sm2O3 catalyst in the production of hydrogen by thermal catalytic decomposition of ammonia, characterized in that: The preparation process of the Ni / SrO-Sm2O3 catalyst is as follows: firstly, soluble Ni salt, Sr salt and Sm salt are dispersed in water and uniformly mixed, and composite hydroxide is obtained by coprecipitation and hydrothermal treatment; then, the composite hydroxide is pyrolyzed at high temperature to obtain composite oxide nanorods; finally, the composite oxide nanorods are treated with high temperature hydrogen to obtain nanorod-shaped Ni / SrO-Sm2O3 catalyst; and then the catalyst is used for thermal catalytic decomposition of ammonia to produce hydrogen.

2. The use according to claim 1, characterized in that: The soluble Ni salt, Sr salt and Sm salt are all their respective nitrates, and the molar ratio of the soluble Ni salt, the soluble Sr salt and the soluble Sm salt is 1:0.5-0.8:0.2-0.

5.

3. The use according to claim 1, characterized in that: The alkali used in the coprecipitation process is one of sodium hydroxide, potassium hydroxide and ammonia water.

4. The use according to claim 1, characterized in that: The temperature of the hydrothermal treatment is 160-200°C and the time is 5-15h.

5. The use according to claim 1, characterized in that: The temperature of the high temperature pyrolysis is 600-700°C and the time is 4-6h.

6. The use according to claim 1, characterized in that: The atmosphere of the high temperature hydrogen treatment is a 6% H2 / Ar mixed atmosphere, the temperature is 550-650°C, and the time is 3-5h.

Citation Information

Patent Citations

  • Catalyst for removing hydrocarbon substances through low-temperature combustion and preparation method thereof

    CN112169787A

  • Rare-earth-based ammonia decomposition catalyst with reversed-phase structure as well as preparation method and application thereof

    CN115920916A

  • Ammonia decomposition catalyst and preparation method and application thereof

    CN117839709A

  • Ammonia decomposing catalyst, ammonia decomposing method using the catalyst, and method for regenerating the catalyst

    JP2012254419A

  • Ammonia-decomposing catalyst

    JP2023074002A