Composite material, preparation method thereof and application of composite material in activating PMS to degrade antibiotics

By introducing oxygen vacancies and growing Co nanoparticles in situ in PMS catalysts, the problems of catalyst stability and degradation efficiency are solved, and efficient antibiotic degradation and easy-to-recover catalysts are achieved. Application in complex water bodies.

CN118976510APending Publication Date: 2024-11-19WUYI UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411120573.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing PMS catalysts have problems such as poor catalyst stability, difficulty in recycling and limited degradation efficiency when degrading antibiotics, especially in complex wastewater systems, which have poor application effects.

Method used

Develop a composite material CoMoO3/MoO3-x, by growing Co nanoparticles in situ and introducing oxygen vacancies, adjusting the electronic structure of cobalt, enhancing catalytic activity, and forming heterojunctions through simple preparation methods to improve the activation capacity of the catalyst and Degradation efficiency.

Benefits of technology

It realizes efficient and stable PMS catalysis, reduces the breaking energy of O-O bonds, improves the generation of active free radicals and the degradation efficiency of pollutants, and the catalyst exhibits high degradation efficiency at low PMS concentrations, and is easy to recycle and reuse. It is suitable for Antibiotic degradation in different water bodies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976510A_ABST
    Figure CN118976510A_ABST
Patent Text Reader

Abstract

The invention discloses a composite material, a preparation method thereof and application of the composite material in activating PMS to degrade antibiotics. The composite material comprises CoMoO3 / MoO3-x and Co nanoparticles growing on the surface of the CoMoO3 / MoO3-x in situ, the CoMoO3 / MoO3-x contains oxygen vacancies, x represents the number of the oxygen vacancies, xgt, and x represents the number of the oxygen vacancies. 0. The composite material disclosed by the invention is rich in active sites, high in catalytic activity, stable in structure in a recycling process, easy to recycle and environment-friendly, and active components are not easy to fall off; according to the invention, a second metal element is introduced to adjust the electronic structure (such as an electron spinning state and local charge density) of cobalt so as to realize a synergistic effect, so that the activation capability of the catalyst on PMS and the degradation efficiency of the catalyst on specific pollutants are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field related to inorganic materials, and in particular to a composite material and a preparation method thereof and application thereof in activating PMS to degrade antibiotics. Background Art

[0002] Antibiotics are one of the typical new pollutants that have attracted widespread attention from all walks of life. Their widespread use and potential risks have aroused deep concern. Metronidazole (MNZ), as a pioneer of nitroimidazole drugs, has occupied an important position in the field of clinical medicine due to its excellent ability to fight against Giardia lamblia, anaerobic bacteria, amoeba trophozoites, Trichomonas vaginalis and other pathogens. In addition, its properties as a highly effective disinfectant have also made it widely used in daily household disinfection and sterilization of public health products.

[0003] However, it cannot be ignored that nitroimidazole drugs, including metronidazole, carry the potential risk of cell mutagenesis and animal carcinogenesis, and due to the stability of their chemical structure, their biodegradation process in the natural environment is extremely slow. What is particularly serious is that animal experiments have clearly revealed the carcinogenic effect of metronidazole on animals. This discovery has prompted countries and regions such as the European Union and the United States to take strict measures to explicitly prohibit the use of such drugs in the production of animal-derived foods to ensure food safety.

[0004] As the research deepens, researchers have found that nitroimidazole drugs such as metronidazole have widely penetrated into natural water bodies and urban sewage treatment systems. Their long-term accumulation not only poses a potential threat to human health, but may also have a long-term impact on the balance and safety of the ecosystem. In view of this, it is particularly important to explore and optimize the treatment technology of pollutants such as metronidazole in water bodies. At present, the treatment strategies for metronidazole in water bodies mainly include three major methods: physical adsorption, biodegradation and chemical transformation. Although physical treatment technology can separate pollutants from water bodies to a certain extent, it faces the limitations of difficulty in recycling and regenerating adsorbent materials and only phase transfer of pollutants without fundamental degradation. Although biological treatment technology is green and environmentally friendly, its treatment efficiency is low and it is easy to induce the spread of resistance genes and strains, so its application is subject to certain restrictions. In contrast, chemical treatment technology, especially advanced oxidation processes (AOPs), has shown strong treatment potential. AOPs activate oxidants to generate highly reactive oxygen species (ROS) through energy input or catalytic action, such as hydroxyl radicals (·OH) and sulfate radicals (SO ) induced by peroxymonosulfate (PMS). 4 · - )、Singlet oxygen( 1 O 2), etc. These strong oxidizing species can undergo complex reactions with antibiotic molecules, including addition, substitution, electron transfer and chemical bond breaking, thereby gradually decomposing the originally difficult-to-biodegrade macromolecular antibiotics into low-toxic or even non-toxic small-molecule compounds, achieving effective degradation and mineralization of pollutants.

[0005] Among the many methods for degrading metronidazole, the permonosulfate (PMS)-based advanced oxidation technology has attracted much attention due to its high efficiency, broad spectrum and thorough degradation, and has become one of the current research hotspots. However, the core challenge of this technology is that it relies on efficient catalysts to activate PMS in order to fully exert its oxidation potential. At present, although some catalyst materials with better performance have shown good results, common problems such as high metal ion dissolution rate, complex preparation process, difficulty in recovery in water environment and short activity duration have seriously restricted the promotion of PMS-based advanced oxidation technology in large-scale industrial applications.

[0006] Cobalt (Co), as a leader among transition metal elements, is widely regarded as one of the key catalysts for activating persulfate (PMS) to generate efficient oxidizing species due to its high redox potential matching with persulfate (PMS), showing extremely high catalytic activity. However, in a typical homogeneous catalytic system, cobalt ions are prone to agglomeration, resulting in high concentrations of ion dissolution, which not only increases the complexity of subsequent processing steps, but also greatly limits the catalyst's recycling capacity and environmental friendliness, thereby limiting its widespread promotion in practical applications.

[0007] To overcome this challenge, researchers have explored a variety of strategies, among which fixing cobalt on matrices such as carbon nanomaterials, porous ceramics or polymer carriers is an effective method. This immobilization technology effectively reduces the dissolution of cobalt ions, improves the stability of the catalyst, and to a certain extent improves the feasibility of its recycling and reuse. Despite this, most current composite support catalysts still exhibit limited degradation efficiency when dealing with complex wastewater systems (such as wastewater containing difficult-to-degrade organic matter such as metronidazole). This is mainly because the interaction mechanism between the carrier and the active metal cobalt needs to be further optimized, and the adaptability of the catalyst in complex environments needs to be improved.

[0008] Therefore, it is very necessary to develop a PMS catalyst that is efficient, stable and easy to recycle. Summary of the invention

[0009] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a composite material that can be used to activate PMS to degrade antibiotics, has the advantages of high efficiency, stability and easy recycling.

[0010] The invention also provides a method for preparing the composite material, and the preparation method is simple and convenient to operate.

[0011] The invention also proposes application of the composite material.

[0012] According to one aspect of the present invention, a composite material is provided, wherein the composite material comprises CoMoO 3 / MoO 3-x and in situ grown on the CoMoO 3 / MoO 3-x Co nanoparticles on the surface, among which CoMoO 3 / MoO 3-x There are oxygen vacancies in it, x represents the number of oxygen vacancies, x>0.

[0013] According to a preferred embodiment of the present invention, at least the following beneficial effects are achieved: the composite material of the present invention has abundant active sites and high catalytic activity. At the same time, the structure is stable and the active components are not easy to fall off during the recycling process, so it is easy to recycle and environmentally friendly. The present invention introduces a second metal element to adjust the electronic structure of cobalt (such as the electron spin state and local charge density, etc.) to achieve a synergistic effect, thereby enhancing the catalyst's ability to activate PMS and its efficiency in degrading specific pollutants. 0 Nanoparticles (NPs) can provide more highly active sites, which show better performance than Co in the active PMS process. 2+ Stronger activity is conducive to reducing the breaking energy barrier of the OO bond, making it easier for OO to break. 2+ It can further participate in the subsequent PMS activation reaction. Therefore, even at low PMS concentrations (≤0.2mM), it can have a high degradation efficiency. At the same time, due to the in-situ growth of cobalt and the introduction of a large number of oxygen vacancies, the Co 2+ The combined effect of oxygen vacancies can accelerate the adsorption process of PMS. The presence of oxygen vacancies can also improve electron transfer and promote the oxidation of organic compounds by singlet oxygen ( 1 O 2 ) is generated. On the other hand, Co 0 Can accelerate Co 3+ To the lower priced Co 2+ The conversion ensures the continuity of the reaction and the formation of the oxidation cycle, overcoming the Co 3+ Compared with other catalysts, the present invention breaks through the disadvantage of Co in traditional Co-based PMS catalysts. 2+ / Co 3+ The activation rate limitation of the redox system significantly increases the generation of active free radicals and the degradation efficiency of pollutants.

[0014] In some embodiments of the invention, 3>x>0.

[0015] In some embodiments of the invention, 1≥x>0.

[0016] In some embodiments of the present invention, the CoMoO 3 / MoO 3-x There is a heterojunction in CoMoO 3 / MoO 3-x The heterojunction formed in the substrate provides a high-speed channel for electron transfer through the cobalt and molybdenum double cycle, greatly improving the degradation efficiency of metronidazole.

[0017] According to another aspect of the present invention, a method for preparing the composite material is provided, comprising the following steps:

[0018] S1, mixing solutions A and B, adding solution C, reacting, separating the reaction product into solid and liquid, and collecting the solid phase, wherein solution A has cobalt salt as solute and organic solvent I as solvent; solution B has molybdate as solute and water as solvent; solution C has 2-methylimidazole as solute and organic solvent II as solvent, and the organic solvents I and II are the same or different;

[0019] S2. Taking the solid phase part and continuously annealing it in an inert atmosphere at 500-900° C. for 3-6 hours to obtain the composite material.

[0020] According to a preferred embodiment of the present invention, the preparation method has at least the following beneficial effects: the preparation method of the present invention is easy to operate and has good industrial application prospects. The composite material of the present invention can synthesize the precursor by a simple room temperature solvent method, and the precursor is subjected to high temperature modification under the protection of an inert atmosphere. The modified material becomes a composite material with rich active sites and high catalytic activity, and at the same time, the structure is stable during recycling and reuse, and the active ingredients are not easy to fall off.

[0021] In some embodiments of the present invention, the annealing temperature in step S2 is 600-800°C.

[0022] In some embodiments of the present invention, the annealing temperature in step S2 is 680-720°C, such as 700°C.

[0023] In some embodiments of the present invention, the temperature is increased at a rate of 5-10° C. / min before annealing in step S2.

[0024] In some embodiments of the present invention, the inert atmosphere is at least one of a nitrogen atmosphere and an Ar atmosphere.

[0025] In some embodiments of the present invention, step S1 comprises adding solution B into solution A.

[0026] In some embodiments of the present invention, the step S1 further comprises stirring the mixed solutions A and B before adding the solution C.

[0027] In some embodiments of the present invention, the stirring speed is 500-700 rpm.

[0028] In some embodiments of the present invention, the stirring speed is 550-650 rpm, preferably 600 rpm.

[0029] In some embodiments of the present invention, the stirring time is 5 to 20 minutes.

[0030] In some embodiments of the present invention, in step S1, the reaction time is 5 to 10 hours.

[0031] In some embodiments of the present invention, in step S1, the reaction is carried out under stirring.

[0032] In some embodiments of the present invention, the stirring speed is 500-700 rpm.

[0033] In some embodiments of the present invention, the stirring speed is 550-650 rpm, preferably 600 rpm.

[0034] In some embodiments of the present invention, the organic solvent I is selected from alcohol solvents, preferably methanol.

[0035] In some embodiments of the present invention, the organic solvent II is selected from alcohol solvents, preferably methanol.

[0036] In some embodiments of the present invention, the molar ratio of the cobalt salt to the molybdate, calculated as Co and Mo, is 1:0.1 to 0.9.

[0037] In some embodiments of the present invention, the molar ratio of the cobalt salt to the molybdate, calculated as Co and Mo, is 1:0.13 to 0.85.

[0038] In some embodiments of the present invention, the molar concentration ratio of the cobalt salt to the molybdate, calculated as Co and Mo, is 1:0.5 to 2.5.

[0039] In some embodiments of the present invention, the molar concentration ratio of the cobalt salt to the molybdate, calculated as Co and Mo, is 1:0.7 to 2.2.

[0040] In some embodiments of the present invention, the molar ratio of the cobalt salt to 2-methylimidazole is 1:0.5-3.5.

[0041] In some embodiments of the present invention, the molar ratio of the cobalt salt to 2-methylimidazole is 1:0.7-3.3.

[0042] In some embodiments of the present invention, the molybdate is ammonium molybdate.

[0043] In some embodiments of the present invention, the preparation method comprises at least one of the following conditions:

[0044] In solution A, Co(NO 3 ) 2 6H 2 The ratio of O and methanol is (1.4-3.5 g):(30-70 mL);

[0045] In solution B, (NH 4 ) 2 MoO 4 ·4H 2 O and deionized water in a ratio of (0.25-0.45 g):(10-50 mL);

[0046] In solution C, the ratio of 2-Methylimidazole to methanol is (1.6-3.8 g):(30-70 mL).

[0047] In some embodiments of the present invention, step S1 further includes the steps of washing and drying the collected solid phase.

[0048] In some embodiments of the present invention, the washing is specifically washing with ethanol for 2 to 4 times.

[0049] In some embodiments of the present invention, the drying is vacuum drying at 60-80°C.

[0050] According to yet another aspect of the present invention, a persulfate catalyst is provided, comprising the above composite material.

[0051] According to a preferred embodiment of the catalyst of the present invention, at least the following beneficial effects are achieved: the persulfate-activated catalyst of the present invention is an environmentally friendly green catalyst, and has broad development space in the field of water treatment technology, especially in the treatment of difficult-to-degrade antibiotics.

[0052] According to another aspect of the present invention, the use of the composite material or the catalyst in activating persulfate to degrade antibiotics is proposed.

[0053] According to another aspect of the present invention, a method for degrading metronidazole-containing wastewater is provided, comprising the following steps: adding the composite material and persulfate to the metronidazole-containing wastewater to be treated.

[0054] In some embodiments of the present invention, the concentration of metronidazole in the metronidazole-containing wastewater to be treated is 10-40 mg / L.

[0055] In some embodiments of the present invention, the composite material is added in a ratio of 5:1-20:1 to the mass concentration of metronidazole in the wastewater.

[0056] In some embodiments of the present invention, the persulfate is added at a concentration of 0.1-0.5 mmol / L.

[0057] In some embodiments of the present invention, the water source of the metronidazole-containing wastewater to be treated is at least one of tap water, deionized water or natural water (such as lake water, river water, etc.). The composite material of the present invention has good adaptability to different water bodies.

[0058] In some embodiments of the present invention, the pH of the metronidazole-containing wastewater to be treated is 2-11. The material has good activation and PMS degradation capabilities within the pH range of 2-11.

[0059] According to another aspect of the present invention, a method for recovering the composite material is provided, comprising the following steps: adsorbing the composite material from the wastewater after degradation by means of a magnet.

[0060] Recycling can be completed through magnetic adsorption, which is easy to operate.

[0061] In the present invention, "CoMoO 3 / MoO 3-x "Represented by CoMoO 3 、MoO 3-x The formed heterojunction nanocomposite material.

[0062] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0064] Figure 1 1 is a SEM image of the composite material prepared in Example 1 of the present invention at different magnifications.

[0065] Figure 2 This is a SEM-EDS characterization result diagram of the composite material prepared in Example 1 of the present invention.

[0066] Figure 3This is a TEM characterization result diagram of the composite material prepared in Example 1 of the present invention.

[0067] Figure 4 This is a graph showing the XRD test results of the composite material prepared in Example 1 of the present invention.

[0068] Figure 5 It is a comparison chart of the test results of the PMS degradation efficiency of the composite material activated by Example 1 of the present invention and the results when only the composite material or only PMS is added.

[0069] Figure 6 It is a comparison chart of the test results of the decomposition efficiency of the composite materials prepared in Examples 1 to 3 of the present invention.

[0070] Figure 7 It is a comparison chart of degradation efficiency test results when the composite material prepared in Example 1 of the present invention is added according to different quality standards.

[0071] Figure 8 It is a comparison chart of the degradation effects of the composite material prepared in Example 1 of the present invention under different pH conditions.

[0072] Fig. 9 This is a comparison chart of the degradation effects of the composite material prepared in Example 1 of the present invention in different water bodies.

[0073] Fig.10 This is a graph showing the recovery performance test results of the composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0074] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of them. Based on the embodiments of the present invention, other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present invention. The test methods used in the embodiments are conventional methods unless otherwise specified; the materials, reagents, etc. used, unless otherwise specified, can be reagents and materials obtained from commercial channels. Unless otherwise specified, the same parameter in each embodiment has the same value. The embodiments described below are exemplary and are only used to explain the present invention, and cannot be understood as limitations on the present invention.

[0075] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0076] Example 1

[0077] In this example, a composite material was prepared, which consisted of CoMoO 3 / MoO 3-x and in situ grown on the CoMoO 3 / MoO 3-x The surface composition of Co nanoparticles (denoted as Co@CoMoO 3 / MoO 3-x ). The specific process is:

[0078] 1. Add 1.4g Co(NO 3 ) 2 6H 2 O was dissolved in 30 mL of methanol to form solution A;

[0079] 2. Add 0.25 g (NH 4 ) 2 MoO 4 ·4H 2 O was dissolved in 10 mL of deionized water to form solution B;

[0080] 3. Dissolve 1.6 g of 2-Methylimidazole in 30 mL of methanol to form solution C;

[0081] 4. After the three liquids are fully dissolved, add solution B to solution A quickly (within 3 seconds), stir at 600 rpm for 15 minutes, then add solution C, continue stirring for 8 hours, and let stand for 11 hours;

[0082] 5. Centrifuge at 5000 rpm, wash with ethanol three times, and collect the pink-purple product;

[0083] 6. The washed material is vacuum dried at 70°C to obtain a precursor;

[0084] 7. Grind the precursor and put it into a porcelain boat, place it in a tube furnace, and anneal it continuously at 700 °C for 4 h at a heating rate of 8 °C / min under a nitrogen atmosphere to obtain Co@CoMoO 3 / MoO 3-x .

[0085] Example 2

[0086] In this example, a composite material was prepared, which consisted of CoMoO 3 / MoO 3-x and in situ grown on the CoMoO 3 / MoO 3-x The surface composition of Co nanoparticles (denoted as Co@CoMoO 3 / MoO 3-x ). The difference between this embodiment and embodiment 1 is that the annealing temperature is 600°C.

[0087] Example 3

[0088] In this example, a composite material was prepared, which consisted of CoMoO 3 / MoO 3-x and in situ grown on the CoMoO 3 / MoO 3-x The surface composition of Co nanoparticles (denoted as Co@CoMoO 3 / MoO 3-x ). The difference between this embodiment and embodiment 1 is that the annealing temperature is 800°C.

[0089] Example 4

[0090] In this example, a composite material was prepared, which consisted of CoMoO 3 / MoO 3-x and in situ grown on the CoMoO 3 / MoO 3-x The surface composition of Co nanoparticles (denoted as Co@CoMoO 3 / MoO 3-x ). The difference between this embodiment and embodiment 1 is that the annealing temperature is 500°C.

[0091] Test example

[0092] This test example tests the morphology, composition and performance of the materials prepared in the examples.

[0093] 1. Morphology characterization

[0094] The morphology of the material prepared in the example was characterized by scanning electron microscopy, wherein the scanning electron microscope (SEM) images of the composite material in Example 1 at different magnifications are as follows: Figure 1 As shown in the figure, it can be seen that the composite material of the present invention has a heterojunction structure of large nanoparticles and regular hexagonal thin sheets. The results of Examples 2 to 4 are similar to those of Examples 2 to 4, which are not shown one by one to avoid redundancy.

[0095] 2. Composition and structure analysis

[0096] The components of the materials prepared in the examples were analyzed by scanning electron microscopy-energy dispersive spectrometer (SEM-EDS), transmission electron microscopy (TEM) and X-ray diffractometer (XRD). The analysis results of Example 1 are as follows: Figures 2 to 4 As shown in the XRD diagram, it can be seen that the material prepared in Example 1 contains Co nanoparticles, CoMoO 3 and MoO 3 , XPS test results show that there is Mo in the surface material 5+ , indicating that there are some oxygen defects. From the TEM characterization results, it can be seen that there is a heterojunction in the composite material of the present invention. The results of Examples 2 to 4 are similar to this, and are not shown one by one to avoid redundancy.

[0097] 3. Analysis of catalytic degradation performance

[0098] Take 100 mL of water sample containing metronidazole at a concentration of 20 mg / L, add 0.02 g of the composite material prepared in Example, 0.02 g of the composite material prepared in Example and 0.03 g of persulfate, and only add 0.03 g of persulfate, respectively, and measure the degradation efficiency within 5 minutes. Take samples once a minute for detection to facilitate the determination of the kinetic constants during the degradation process. The degradation effect of the composite material prepared in Example 1 is as follows: Figure 5 As shown in the figure, it can be seen that 99% of metronidazole can be degraded in 3 minutes, and its performance is better than most reported PMS activators. However, among the single Co-based catalyst materials prepared by conventional methods, it can only degrade 24% of metronidazole within 5 minutes. By comparing the pseudo-first-order rate constant k value, the composite material in Example 1 of the present invention has a k value of up to 1.4663 min when activating persulfate to degrade metronidazole. -1 , which is 18.3 times that of the single Co-based catalyst system, and the Co ion dissolution rate is much lower than that of the single Co-based system. In addition, the catalyst can also degrade 99% of metronidazole within 5 minutes after recycling and reuse. It has high efficiency and stability, and can respond quickly and effectively to PMS activators in a variety of complex actual water bodies.

[0099] The composite materials in Examples 2 to 4 also have good catalytic degradation activity. The catalytic degradation effects in Examples 1 to 3 are summarized as follows: Figure 6 As shown in the figure, it can be seen that the catalytic degradation effect of Example 1 is the best, Example 2 is close to it, and Example 3 is slightly lower, but the degradation can still be basically completed within 4 minutes.

[0100] Furthermore, the catalytic degradation effect when the composite material was added at different ratios (0.05 g / L, 0.1 g / L, 0.2 g / L, 0.3 g / L) was also tested. The test results of the composite material of Example 1 are as follows: Figure 7As shown in the figure, it can be seen that with the increase of the addition amount, the catalytic degradation efficiency increases, but when the addition amount exceeds 0.2g / L, the increase in catalytic degradation efficiency decreases.

[0101] Furthermore, the catalytic degradation effect of the composite material in water systems under different pH conditions was also tested. The test results of the composite material of Example 1 are as follows: Figure 8 As shown in the figure, it can be seen that the material of the scheme of the present invention has good activation and PMS degradation ability in the pH range of 2-11.

[0102] In addition, the catalytic degradation effect in different water bodies was also tested. Metronidazole was added to water bodies from different sources. The test results of the composite material prepared in Example 1 are as follows: Fig. 9 As shown in the figure, it can be seen that the material of the scheme of the present invention has good adaptability to different water bodies and can respond quickly and effectively to the PMS activator in a variety of complex actual water bodies.

[0103] 4. Recycling performance analysis

[0104] The prepared composite material is tested for its recycling performance. After the adsorption degradation is completed, the composite material is adsorbed and recovered from the wastewater after the degradation by a magnet.

[0105] The test results of the recycling performance of the composite material prepared in Example 1 are as follows: Fig.10 As shown in the figure, it can be seen that the material still has a high activated PMS degradation efficiency after three cycles of use. Even after recycling and reuse, it can degrade 99% of metronidazole within 5 minutes, which is highly efficient and stable.

[0106] In summary, the composite material of the present invention after modification becomes a composite material with rich active sites and high catalytic activity, and at the same time, the structure is stable and the active ingredients are not easy to fall off during recycling. The in-situ formation of Co nanoparticles during the exsolution phase transition can provide more high-activity sites, which shows a better performance than Co in the activation of PMS. 2+ It has stronger activity, which is beneficial to reduce the breaking energy barrier of the OO bond, making it easier for OO to break. 2+ It can further participate in the subsequent PMS activation reaction. After high temperature treatment, the active sites are exposed on the catalyst surface and evenly dispersed, and the Co with stronger reduction activity 0 The introduction of 2+ / Co 3+ The activation rate of the redox system is limited. At the same time, the synergistic effect of the Co site and the surrounding oxygen vacancies can break the O─H bond of the PMS molecule, generating a large amount of 1 O 2 and SO4 - Active substance: CoMoO 3 / MoO 3-x The formed heterojunction serves as a substrate to provide a high-speed channel for electron transfer through a double cycle of cobalt and molybdenum, greatly improving the degradation efficiency of metronidazole. The material has good activated PMS degradation ability in the pH range of 2-11. The material is recycled and reused and it is found that the material still has a high activated PMS degradation efficiency after three cycles of use. This shows that the material of the scheme of the present invention is not only environmentally friendly, but also has broad development space in the field of water treatment technology, especially in the treatment of difficult-to-degrade antibiotics.

[0107] The embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A composite material, characterized in that: The composite material includes CoMoO3 / MoO 3-x and in situ grown on the CoMoO3 / MoO 3-x Co nanoparticles on the surface, among which CoMoO3 / MoO 3-x There are oxygen vacancies in it, x represents the number of oxygen vacancies, x>0.

2. The composite material according to claim 1, characterized in that: The CoMoO3 / MoO 3-x There is a heterojunction in it.

3. The method for preparing a composite material according to claim 1 or 2, characterized in that: The steps include: S1, mixing solutions A and B, adding solution C, reacting, separating the reaction product into solid and liquid and collecting the solid phase, wherein solution A has cobalt salt as solute and organic solvent I as solvent; solution B has molybdate as solute and water as solvent; solution C has 2-methylimidazole as solute and organic solvent II as solvent, and the organic solvents I and II are the same or different; S2. Taking the solid phase part and continuously annealing it in an inert atmosphere at 500-900° C. for 3-6 hours to obtain the composite material.

4. The preparation method according to claim 3, characterized in that: The annealing temperature in step S2 is 600-800°C; preferably, the annealing temperature in step S2 is 680-720°C.

5. The preparation method according to any one of claims 3 to 4, characterized in that: In step S1, at least one of the following conditions is met: 1) The organic solvent I is selected from methanol; and / or, the organic solvent II is selected from methanol; 2) The molar ratio of the cobalt salt to the molybdate, calculated as Co and Mo, is 1:0.1 to 0.9; preferably 1:0.13 to 0.85; 3) The molar concentration ratio of the cobalt salt to the molybdate, calculated as Co and Mo, is 1:0.5 to 2.5; preferably 1:0.7 to 2.2; 4) The molar ratio of the cobalt salt to 2-methylimidazole is 1:0.5-3.5; preferably 1:0.7-3.

3.

6. A persulfate catalyst, characterized in that: Comprising the composite material as claimed in claim 1 or 2.

7. Use of the composite material according to claim 1 or 2 or the catalyst according to claim 6 in activating persulfate to degrade antibiotics.

8. A method for degrading wastewater containing metronidazole, characterized in that: The method comprises the following steps: adding the composite material and persulfate as claimed in claim 1 or 2 into the metronidazole-containing wastewater to be treated.

9. The method for degrading metronidazole-containing wastewater according to claim 8, characterized in that: The water source of the metronidazole-containing wastewater to be treated is at least one of tap water, deionized water or natural water; and / or the pH of the metronidazole-containing wastewater to be treated is 2-11.

10. A method for recycling a composite material as claimed in claim 1 or 2, characterized in that: The method comprises the following steps: adsorbing the composite material from the waste water after the degradation is completed by using a magnet.

Citation Information

Patent Citations

  • Cobalt oxide / molybdenum oxide graded heterostructure nanosheet and preparation method thereof

    CN108598399A

  • Nitrogen-doped carbon-coated non-noble bimetal cobalt molybdenum oxide oxygen evolution reaction catalyst, and preparation method and application thereof

    CN112553643A

  • Cobalt-molybdenum alloy and cobalt-molybdenum mixed oxide electrocatalyst and preparation method and application thereof

    CN113621987A

  • Preparation method and application of porous nano cobaltosic oxide

    CN114835171A

  • Molybdenum trioxide composite material and preparation method and application thereof