Ultrathin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst and preparation method thereof
By constructing a double heterostructure of ultra-thin carbon nitride-bismuth iodine-bismuth sulfide composite photocatalyst, the problem of low efficiency of pure graphite phase carbon nitride photocatalyst is solved, and efficient photocatalytic performance and stability are achieved, significantly Improve the efficiency of pollutant degradation.
Patent Information
- Application Number
- CN202411034864.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The efficiency of pure graphite phase carbon nitride (g-C3N4) in photocatalytic degradation of pollutants is limited by the rapid recombination of photogenerated electron holes and low quantum efficiency, which limits the development of its application fields.
Ultrathin carbon nitride-bismuth iodine-bismuth sulfide composite photocatalyst was constructed, and a double heterostructure was formed by mechanical ball milling method, which improved the separation efficiency of electron-hole pairs and the stability of the catalyst, and ions were caused by Na2S·9H2O. Exchanges form Bi2S3 nanosheets to form a two-dimensional ultra-thin structure to improve catalytic performance.
The photocatalytic performance and the stability of the catalyst are significantly improved, and the efficiency of the catalyst in degrading dyes is increased by 7.9 times, forming excellent photocatalytic performance, which can effectively degrade organic pollutants.
Smart Images

Figure CN118976522A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalytic degradation, and specifically relates to an ultra-thin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst and a preparation method thereof. Background Art
[0002] With the acceleration of industrialization and urbanization, the emission and accumulation of various organic pollutants have caused serious environmental pollution problems. These organic pollutants have caused obvious harm to the environment and ecosystem, and also brought potential dangers to human health. Traditional pollutant treatment methods, such as biological decomposition, chemical oxidation and physical adsorption, are usually limited by low treatment efficiency, high cost, by-product generation and complex operation. Therefore, it has become more important to find effective, economical and environmentally friendly pollution treatment methods.
[0003] Graphitic carbon nitride (g-C3N4) has the characteristics of two-dimensional (2D) graphene-like nanosheet structure, strong visible light absorption, narrow band gap, easy structural modification, good charge transfer ability and low preparation cost. It is a new type of non-metallic semiconductor photocatalyst that responds to visible light. It has been widely used in photocatalytic degradation of pollutants and photocatalytic hydrogen production. However, the photocatalytic efficiency of pure g-C3N4 is limited by the rapid recombination of photogenerated electrons and holes and low quantum efficiency, which restricts its development in application fields. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes an ultra-thin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst and a preparation method thereof, constructs a double heterostructure, so that the separation efficiency of electron-hole pairs is higher, and the photocatalytic performance and stability of the catalyst are also higher.
[0005] In order to achieve the above object, the present invention is achieved through the following technical solutions:
[0006] An ultra-thin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst comprises g-C3N4, BiOI and Bi2S3, wherein the g-C3N4, BiOI and Bi2S3 together form a double heterostructure.
[0007] The present invention also provides a method for preparing the composite photocatalyst, comprising the following steps:
[0008] S1: Preparation of g-C3N4 catalyst: melamine powder is heated and calcined, and after cooling to room temperature, it is taken out and ground into powder to obtain light yellow g-C3N4;
[0009] S2: Preparation of BiOI catalyst: Bi(NO3)·5H2O and KI were uniformly dispersed in a mixture of deionized water and ethylene glycol, stirred to react until a red product was formed, then washed and centrifuged, and dried to obtain blocky BiOI, which was ground to obtain orange powdery BiOI;
[0010] S3: Preparation of U-C3N4 / BiOI / Bi2S3 catalyst: g-C3N4 and BiOI were placed in a ball mill at a ratio of 1:0.05, and Na2S·9H2O solution was added. The mixture was ball milled and centrifuged to obtain U-C3N4 / BiOI / Bi2S3 catalyst.
[0011] Preferably, in S1, melamine powder is put into a porcelain boat, and placed in a muffle furnace, and the temperature is increased to 550° C. at a heating rate of 5° C. / min, and maintained at this temperature for 4 hours.
[0012] Preferably, the molar ratio of Bi(NO3)·5H2O to KI in S2 is 1:1.
[0013] Preferably, the ratio of deionized water to ethylene glycol solution in S2 is 5:1.
[0014] Preferably, in S2, 2 mmol of Bi(NO3)˙5H2O and 2 mmol of KI are uniformly dispersed in a uniform mixture of 100 mL of deionized water and 20 mL of ethylene glycol, and stirred at room temperature for 3 h until a red product is formed, and then washed with deionized water and ethanol for multiple times and centrifuged, and finally dried in a drying oven at 60°C overnight, and the obtained blocky BiOI is then ground to finally obtain orange powder BiOI.
[0015] Preferably, g-C3N4 and BiOI are placed in a ball mill at a ratio of 1:0.05 in S3, a Na2S·9H2O solution with a concentration of 0.7 g / L is added, and deionized water is added for ball milling. The speed of the ball mill is 400 r / min. -1 The ball milling time was 18 hours. After grinding, it was filtered, then washed with deionized water and ethanol several times and centrifuged to dry, and finally a gray U-C3N4 / BiOI / Bi2S3 catalyst powder was obtained.
[0016] Finally, the present invention also provides the use of the composite photocatalyst prepared by the above method in degrading organic pollutants.
[0017] The beneficial effects of the present invention are:
[0018] The present invention successfully constructs a double heterostructure by mechanical ball milling, so that the separation efficiency of electron-hole pairs is higher, the photocatalytic performance and the stability of the catalyst are also higher, and secondly, the catalyst is formed into a two-dimensional ultra-thin structure by ball milling, and this fine ultra-thin layered structure can better contact with the reaction medium, and also provide more active sites for the reaction, and in addition, during the ball milling process, Na2S·9H2O is added to cause ion exchange on BiOI, thereby successfully forming Bi2S3 on the BiOI nanosheet. This catalyst has excellent photocatalytic performance and can play an important role in degrading dyes. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0020] Figure 1 This is the high-resolution TEM image of U-C3N4 / BiOI / Bi2S3 in Example 1.
[0021] Figure 2 This is the AFM image of U-C3N4 / BiOI / Bi2S3 in Example 1.
[0022] Figure 3 This is a photocatalytic degradation effect diagram of methylene blue by U-C3N4 / BiOI / Bi2S3 in Example 1 and g-C3N4 and BiOI in Comparative Example 1.
[0023] Figure 4 XRD spectra of U-C3N4 / BiOI / Bi2S3 in Example 1 and g-C3N4 and BiOI in Comparative Example 1. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0025] Example 1
[0026] Preparation of U-C3N4 / BiOI / Bi2S3 catalyst:
[0027] S1: Put 5g of melamine into a porcelain boat and wrap it evenly with tin foil to prepare for subsequent uniform heating. Then put the porcelain boat into a muffle furnace and heat it at a heating rate of 5 degrees Celsius per minute until the temperature reaches 550 degrees Celsius. After keeping this temperature for 4 hours, cool the muffle furnace to room temperature, then take out the porcelain boat, take out the product in the porcelain boat and put it into a mortar for grinding. After it is ground into a uniform and fine powder, the initial light yellow g-C3N4 is finally obtained.
[0028] S2: Weigh 0.97g (2mmol) of Bi(NO3)˙5H2O and 0.33g (2mmol) of KI into a 250mL beaker, add 100mL of deionized water and 20mL of ethylene glycol to mix them evenly, then place the beaker on a magnetic stirrer and stir at room temperature for 3 hours. At this time, a red product is formed. The product is then washed three times with deionized water and ethanol and centrifuged, and finally dried in a drying oven at 60 degrees Celsius overnight. The resulting blocky BiOI is ground again with a mortar to finally obtain orange powder BiOI.
[0029] S3: The prepared g-C3N4 and BiOI were placed in a zirconia ball mill with different sizes in a ratio of 1:0.05. Here, 1g of g-C3N4 and 0.05g of BiOI were selected. Then, a solution of 0.7g / L Na2S·9H2O was added, and then 30mL of deionized water was added for wet grinding. The speed of the ball mill was 400r / min. -1 The ball milling time was 18 hours. The ground product was filtered with a sieve, and then washed three times with deionized water and ethanol and centrifuged to dry, finally obtaining a gray powder U-C3N4 / BiOI / Bi2S3 catalyst. The high-resolution TEM image of the U-C3N4 / BiOI / Bi2S3 catalyst is shown in FIG. Figure 1 As shown in the AFM image, Figure 2 shown.
[0030] 50 mg of the photocatalyst U-C3N4 / BiOI-5 / Bi2S3 was evenly dispersed in 100 mL of a methylene blue solution with a concentration of 10 mg / L. A 300 W xenon lamp was used to simulate sunlight, and a cutoff filter with λ>420 nm was used. The cooling circulating water was turned on to maintain room temperature.
[0031] Comparative Example 1
[0032] 50 mg of photocatalyst g-C3N4 and BiOI were uniformly dispersed in 100 mL of methylene blue solution with a concentration of 10 mg / L. A 300 W xenon lamp light source was used to simulate sunlight, and a cutoff filter of λ>420 nm was used. At the same time, the cooling circulating water needed to be turned on to maintain room temperature.
[0033] The degradation of Example 1 is compared with that of Comparative Example 1. Figure 3 Photocatalytic degradation of methylene blue Figure 4 As shown in the XRD spectra of U-C3N4 / BiOI / Bi2S3, g-C3N4 and BiOI, the results show that the degradation efficiency of the catalyst U-C3N4 / BiOI / Bi2S3 is 7.9 times higher than that of g-C3N4 before composite and 4.6 times higher than that of BiOI, which indicates that the successful composite and ultra-thin structure of the ternary heterojunction are helpful to improve the degradation performance of g-C3N4.
[0034] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all details in detail, nor do they limit the invention to only the specific embodiments described. Obviously, many modifications and changes can be made according to the content of this specification.
Claims
1. A method for preparing an ultrathin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst, characterized in that: The following steps are involved: S1: Preparation of g-C3N4 catalyst: melamine powder is heated and calcined, and after cooling to room temperature, it is taken out and ground into powder to obtain light yellow g-C3N4; S2: Preparation of BiOI catalyst: Bi(NO3)·5H2O and KI were uniformly dispersed in a mixture of deionized water and ethylene glycol, stirred to react until a red product was formed, then washed and centrifuged, and dried to obtain blocky BiOI, which was ground to obtain orange powdery BiOI; S3: Preparation of U-C3N4 / BiOI / Bi2S3 catalyst: g-C3N4 and BiOI were placed in a ball mill at a ratio of 1:0.05, and Na2S·9H2O solution was added. The mixture was ball milled and centrifuged to obtain U-C3N4 / BiOI / Bi2S3 catalyst.
2. The method for preparing the ultrathin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst according to claim 1, characterized in that: In S1, the melamine powder is heated to 550° C. at a heating rate of 5° C. / min and maintained at this temperature for 4 hours.
3. The method for preparing the ultrathin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst according to claim 1, characterized in that: The molar ratio of Bi(NO3)·5H2O to KI in the S2 is 1:
1.
4. The method for preparing the ultrathin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst according to claim 3, characterized in that: The ratio of deionized water to ethylene glycol solution in S2 is 5:
1.
5. The method for preparing the ultrathin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst according to claim 4, characterized in that: In the S2, 2 mmol Bi(NO3)˙5H2O and 2 mmol KI are uniformly dispersed in a uniform mixture of 100 mL deionized water and 20 mL ethylene glycol, and stirred for 3 h at room temperature until a red product is formed. The product is then washed with deionized water and ethanol multiple times and centrifuged. Finally, the product is dried in a drying oven at 60°C overnight. The obtained blocky BiOI is then ground to obtain an orange powder BiOI.
6. The method for preparing the ultrathin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst according to claim 1, characterized in that: In the S3, g-C3N4 and BiOI are placed in a ball mill at a ratio of 1:0.05, a Na2S·9H2O solution with a concentration of 0.7 g / L is added, and deionized water is added for ball milling. The speed of the ball mill is 400 r / min. -1 The ball milling time was 18 hours. After grinding, it was filtered, then washed with deionized water and ethanol several times and centrifuged to dry, and finally a gray U-C3N4 / BiOI / Bi2S3 catalyst powder was obtained.
7. Use of the ultrathin carbon nitride-bismuth oxyiodide-bismuth sulfide composite photocatalyst according to any one of claims 1 to 6 in degrading organic pollutants.
Citation Information
Patent Citations
Cake-shaped Bi2S3 thermoelectric material and preparation method thereof
CN113666416A
Three-dimensional porous graphite phase carbon nitride / bismuth oxyiodide / silver nanoparticle composite photocatalyst as well as preparation method and application thereof
CN114522709A
Preparation method and application of molecularly imprinted BiOI / g-carbon nitride catalyst
CN117443426A