Nitrogen-doped biomass charcoal / transition metal catalyst as well as preparation method and application thereof

Through the preparation method of nitrogen-doped biomass carbon/transition metal catalyst, the problems of high cost and low selectivity of existing catalysts in the coal tar conversion process are solved, and efficient preparation of light aromatic hydrocarbons is achieved, which is suitable for large-scale applications.

CN118976523AActive Publication Date: 2024-11-19YUNNAN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411040713.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

In the process of converting coal tar into light aromatic hydrocarbons, existing catalysts have problems such as high cost, complex processes, low yields and insufficient selectivity. In particular, Ni-based catalysts are prone to carbon accumulation and have poor durability, making it difficult to achieve efficient conversion under harsh conditions.

Method used

Using the preparation method of nitrogen-doped biomass carbon/transition metal catalyst, catalysts with high specific surface area and optimized charge distribution are prepared by waste biomass calcination, nitrogen doping treatment and transition metal loading, combined with hydrothermal reaction and hydrogen calcination. .

Benefits of technology

It achieves efficient catalytic pyrolysis under hydrogen-free and solvent-free conditions, improves the tar conversion rate and selectivity of light aromatic hydrocarbons, and is simple in process and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976523A_ABST
    Figure CN118976523A_ABST
Patent Text Reader

Abstract

The invention discloses a nitrogen-doped biomass charcoal / transition metal catalyst as well as a preparation method and application thereof, and belongs to the technical field of catalysts. The method comprises the following steps: calcining waste biomass in an inert atmosphere to obtain biomass charcoal; the preparation method comprises the following steps: calcining biomass charcoal, melamine and potassium hydroxide in a CO2 atmosphere to obtain nitrogen-doped biomass charcoal, then adding the nitrogen-doped biomass charcoal into a transition metal salt solution for dipping, and then carrying out hydrothermal treatment; and finally, reducing the mixture obtained by the hydrothermal method in a hydrogen atmosphere to obtain the nitrogen-doped carbon / transition metal catalyst. The nitrogen-doped carbon transition metal catalyst provided by the invention has the advantages of high selectivity, high conversion rate, mild reaction conditions, high light aromatic hydrocarbon selectivity, safe operation and simple process in preparation of aromatic hydrocarbon through catalytic pyrolysis of coal tar.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts, and in particular relates to a nitrogen-doped biochar / transition metal catalyst and a preparation method and application thereof. Background Art

[0002] With the rapid development of my country's economy, the problem of energy consumption is becoming increasingly serious. Coal is regarded as one of the most important fossil energy sources in my country due to its abundant reserves and wide distribution range. However, a large amount of coal tar will be produced during the pyrolysis or gasification of coal. Coal tar is a valuable resource, and with the increase of its production capacity, the need for large-scale utilization is becoming more and more urgent. However, coal tar has the characteristics of poor chemical stability, poor thermal stability, high viscosity, corrosiveness and density, which greatly limits its application. Therefore, it is necessary to convert coal tar into chemicals or hydrocarbon fuels. Light aromatics, especially benzene, toluene, xylene, trimethylbenzene and naphthalene, are widely used as raw materials for important chemical products such as synthetic rubber, resin, fiber, medicine, dye and gasoline additives. However, the CC bond in coal tar is very stable, which usually requires its conversion to overcome the reaction thermodynamic and kinetic barriers under harsh conditions. Hydrocracking can be used to refine coal tar and obtain high-content aromatics. However, existing research mainly uses hydrogenation, pressurization and external catalysts to achieve the conversion of coal tar into aromatics. The process is complicated and consumes a large amount of co-reactants such as hydrogen and solvents.

[0003] CN107537477A discloses a Pt / TiO2 catalyst, which has a complicated preparation process, uses precious metal Pt as an active component, and uses rare metal TiO2 as a carrier, which has a high preparation cost and is not suitable for large-scale application. CN105536860A discloses a Ni2P / Zr-MCM41 catalyst and a preparation method thereof, which has a complicated preparation process, harsh conditions, releases highly toxic phosphine during the preparation process, and takes a long time to prepare, and the preparation method needs to be further improved.

[0004] In recent years, catalytic pyrolysis technology has been recognized as an effective strategy for activating CC bonds due to its high tar conversion rate and low cost advantages. However, most catalysts only show excellent monofunctional catalytic activity and cannot simultaneously achieve the conversion of aliphatic hydrocarbons and polycyclic aromatic hydrocarbons in coal tar to light aromatic hydrocarbons. Ni-based catalysts have become the catalysts with the most promising industrial applications due to their low price and similar catalytic activity to precious metals. However, Ni-based catalysts have problems of easy carbon deposition and durability, and are easily oxidized. In recent years, although nanocatalysts based on d-block transition metals (especially Fe, Co and Ni) anchored on nitrogen-doped carbon substrates have attracted much attention, the high surface energy of Ni metal easily induces catalyst agglomeration, resulting in great challenges in the precise preparation of highly active Ni-based catalytic systems. In addition, due to the complexity of real coal tar components, current catalysts still face problems such as low aromatic yield and light aromatic selectivity. To this end, the present invention uses waste biomass as a template and carbon source to prepare a nitrogen-doped carbon / transition metal catalyst for catalytic pyrolysis of coal tar to prepare aromatic hydrocarbons. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a nitrogen-doped biochar / transition metal catalyst and a preparation method and application thereof.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a nitrogen-doped biochar / transition metal catalyst comprises the following steps:

[0008] (1) calcining the waste biomass under an inert gas to obtain biochar, then adding a nitrogen source and a strong base to mix evenly, calcining under CO2 gas, and finally washing and drying to obtain nitrogen-doped biochar;

[0009] (2) Immersing the nitrogen-doped biochar in a transition metal salt solution, stirring, and ultrasonicating, and then sequentially performing a hydrothermal reaction, drying, and calcining under hydrogen to obtain a nitrogen-doped biochar / transition metal catalyst.

[0010] As a preferred embodiment of the present invention, the waste biomass is one of wheat straw, tobacco stems, pine needles and corn straw.

[0011] As a preferred embodiment of the present invention, in step (1), the waste biomass is calcined under inert gas at a temperature of 550-900°C, a time of 1-2h, a heating rate of 10-40°C / min, and a flow rate of the inert gas of 20-150ml / min.

[0012] The inert gas is one of nitrogen, argon and helium.

[0013] As a preferred embodiment of the present invention, in the step (1), the calcination temperature under CO2 gas is 600-900°C, the time is 1-3h, the concentration of CO2 is 5% to 100%, and the flow rate is 20 to 150mL / min.

[0014] Compared with inert gas, calcination in CO2 in step (2) of the present invention is beneficial to the activation of biochar. The prepared biochar has a more developed pore size, a larger specific surface area, and a richer defect structure. Most importantly, it is beneficial to the loading and dispersion of transition metal active components, making the catalyst more active.

[0015] As a preferred embodiment of the present invention, the nitrogen source is at least one of melamine, urea, and polyethylene glycol; the strong base is one of sodium hydroxide, potassium hydroxide, and calcium hydroxide; and the mass ratio of the biochar, the nitrogen source, and the strong base is 2-5:0.2-0.8:1-5.

[0016] The invention prepares nitrogen-doped biochar by means of two-step calcination of waste wheat straw, melamine and potassium hydroxide, thereby overcoming the disadvantage that the nitrogen-doped biochar prepared by one-step calcination of waste wheat straw, melamine and potassium hydroxide is not conducive to the loading and dispersion of the transition metal active phase, resulting in low activity of the catalyst.

[0017] As a preferred embodiment of the present invention, the transition metal salt is at least one of nickel nitrate, cobalt nitrate, iron nitrate and copper nitrate, and the mass of the transition metal salt is 1-10% of the mass of the nitrogen-doped biochar.

[0018] As a preferred embodiment of the present invention, in the step (2), the stirring time is 10-30 min, the ultrasonic time is 20-40 min; the temperature of the hydrothermal reaction is 150-300° C., and the time is 12-24 h.

[0019] The present invention adopts hydrothermal reaction to make the prepared catalyst more conducive to the adsorption and activation of coal tar components, and the activity and stability of the catalyst are better. If the hydrothermal reaction is lacking, the aromatic yield and light aromatic selectivity of the prepared material are significantly reduced, and the performance stability of the material is also significantly reduced.

[0020] As a preferred embodiment of the present invention, in the step (2), the calcination temperature under hydrogen is 700-900°C, the time is 30-120 min, the concentration of hydrogen is 3%-100%, and the flow rate is 50-100 mL / min.

[0021] The present invention also claims protection for the nitrogen-doped carbon / transition metal catalyst prepared by the preparation method of the nitrogen-doped carbon / transition metal catalyst.

[0022] The present invention also claims to protect the use of the nitrogen-doped carbon / transition metal catalyst in the preparation of aromatic hydrocarbons by catalytic pyrolysis of coal tar.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: the preparation method of the nitrogen-doped biomass carbon / transition metal catalyst of the present invention is simple in process and suitable for large-scale production, and the prepared nitrogen-doped carbon / transition metal catalyst has a large specific surface area, nitrogen doping and transition metal improve the defect structure of the catalyst, promote electron transfer, and optimize the charge distribution of the catalyst, the transition metal particles are small in size and evenly distributed, and can realize the catalytic pyrolysis of coal tar to prepare light aromatics under hydrogen-free and solvent-free conditions, reflecting high tar conversion rate and high light aromatics selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the component distribution diagram of coal tar.

[0025] Figure 2 Flow chart of the preparation of nitrogen-doped biochar / transition metal catalysts.

[0026] Figure 3 TEM images of the catalysts prepared in Example 2 and Comparative Example 3, wherein Figure (a) is the TEM image of the biochar / transition metal catalyst prepared in Comparative Example 3, Figure (b) is the TEM image of the nitrogen-doped biochar / transition metal catalyst prepared in Example 2, and Figure (c) is the HRTEM image of the nitrogen-doped biochar / transition metal catalyst prepared in Example 2.

[0027] Figure 4 The XRD diagrams of the catalysts prepared in Example 2 and Comparative Examples 1-3.

[0028] Figure 5 The Raman graphs of the catalysts prepared in Example 2 and Comparative Examples 1-3. DETAILED DESCRIPTION

[0029] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0030] Example 1

[0031] A method for preparing a nitrogen-doped biochar / transition metal catalyst comprises the following steps:

[0032] (1) The discarded wheat straw was crushed and sieved into 60-80 mesh, added into deionized water, stirred and washed for 12 h, dried in a 105 °C forced air drying oven for 12 h, and calcined at 750 °C for 1 h (heating rate: 10 °C / min) under nitrogen gas with a nitrogen flow rate of 50 mL / min to obtain biochar.

[0033] (2) Add 0.2 g of melamine and 4.0 g of potassium hydroxide to 2 g of biochar and grind them thoroughly. Then, calcine them under 10% CO2 gas for 1 h (heating rate: 10°C / min) with a CO2 flow rate of 50 mL / min. After cooling, filter and wash them several times with deionized water, and dry them in a 105°C forced air drying oven for 12 h to obtain nitrogen-doped biochar.

[0034] (3) The nitrogen-doped biochar was added to a pre-prepared nickel nitrate solution (the mass fraction of nickel relative to the nitrogen-doped biochar was 2%) and stirred for 15 minutes, ultrasonically impregnated for 15 minutes, and then the impregnated mixture was transferred to an autoclave and heat treated at 250°C for 12 hours. After cooling, the mixture was dried in a 105°C forced air drying oven for 24 hours.

[0035] (4) The solid obtained in step (3) was calcined and reduced in a 15% hydrogen atmosphere (hydrogen flow rate: 50 mL / min) using a tubular furnace (heating rate: 10°C / min) for 1 h to obtain a nitrogen-doped biochar / transition metal catalyst.

[0036] Example 2

[0037] The only difference between the preparation method of a nitrogen-doped biochar / transition metal catalyst in this embodiment and that in Embodiment 1 is that in step (3), the nitrogen-doped biochar is added to a pre-prepared nickel nitrate solution, and the mass fraction of nickel relative to the nitrogen-doped biochar is 5%.

[0038] according to Figure 3 It can be seen that compared with the biochar / nickel catalyst in Comparative Example 3, the nickel in the nitrogen-doped carbon-nickel catalyst prepared in Example 2 has better dispersibility, and the nickel exists in the form of elemental nickel. Figure 4 It can be seen that there is zero-valent nickel metal in the nitrogen-doped carbon / nickel catalyst, and the intensity of the nickel diffraction peak in the nitrogen-doped carbon-nickel catalyst is lower than that in the biomass carbon-nickel catalyst, indicating that nitrogen doping increases the defects of the catalyst, which is conducive to the formation of nickel nanoparticles, and Figure 5 Raman analysis showed that the I D / I G (0.99) The intensity ratio is higher than that of the biomass carbon nickel catalyst (0.95), indicating that it has more defects, which is beneficial to increase the active sites in the tar conversion process.

[0039] Example 3

[0040] The only difference between the preparation method of a nitrogen-doped biochar / transition metal catalyst in this embodiment and that in Embodiment 1 is that in step (3), the nitrogen-doped biochar is added to a pre-prepared ferric nitrate solution, and the mass fraction of iron relative to the nitrogen-doped biochar is 5%.

[0041] Example 4

[0042] The only difference between the preparation method of a nitrogen-doped biochar / transition metal catalyst in this embodiment and that in Embodiment 1 is that in step (3), the nitrogen-doped biochar is added to a pre-prepared cobalt nitrate solution, and the mass fraction of cobalt relative to the nitrogen-doped biochar is 5%.

[0043] Example 5

[0044] The only difference between the preparation method of a nitrogen-doped biochar / transition metal catalyst in this embodiment and that in Embodiment 1 is that in step (3), the nitrogen-doped biochar is added to a pre-prepared copper nitrate solution, and the mass fraction of copper relative to the nitrogen-doped biochar is 5%.

[0045] Example 6

[0046] A method for preparing a nitrogen-doped biochar / transition metal catalyst comprises the following steps:

[0047] (1) The tobacco stems were crushed and sieved into 60-80 mesh, added into deionized water, stirred and washed for 6 h, dried in a forced air drying oven at 80 °C for 24 h, and calcined at 900 °C for 2 h (heating rate: 40 °C / min) under nitrogen gas with a nitrogen flow rate of 150 mL / min to obtain biochar.

[0048] (2) Add 0.8 g polyethylenediamine and 1.0 g sodium hydroxide to 5 g of biochar and grind them thoroughly. Then, calcine them under 5% CO2 gas for 3 h (heating rate: 40°C / min) with a CO2 flow rate of 20 mL / min. After cooling, filter and wash them several times with deionized water, and dry them in a forced air drying oven at 80°C for 24 h to obtain nitrogen-doped biochar.

[0049] (3) The nitrogen-doped biochar was added to a pre-prepared nickel nitrate solution (the mass fraction of nickel relative to the nitrogen-doped biochar was 10%) and stirred for 30 minutes, ultrasonically impregnated for 20 minutes, and then the impregnated mixture was transferred to an autoclave and heat treated at 150°C for 24 hours. After cooling, the mixture was dried in an 80°C forced air drying oven for 12 hours.

[0050] (4) The solid obtained in step (3) was calcined and reduced in a 3% hydrogen atmosphere (hydrogen flow rate: 100 mL / min) using a tubular furnace (heating rate: 40°C / min) for 1 h to obtain a nitrogen-doped biochar / transition metal catalyst.

[0051] Example 7

[0052] A method for preparing a nitrogen-doped biochar / transition metal catalyst comprises the following steps:

[0053] (1) The pine needles were crushed and sieved into 60-80 mesh, added into deionized water, stirred and washed for 6 h, dried in a 90 °C forced air drying oven for 20 h, and calcined at 550 °C for 1.5 h (heating rate: 20 °C / min) under nitrogen gas with a nitrogen flow rate of 20 mL / min to obtain biochar.

[0054] (2) Add 0.5 g urea and 5.0 g calcium hydroxide to 3 g biochar and grind them thoroughly. Then calcine them under 100% CO2 gas for 3 h (heating rate: 20 °C / min) with a CO2 flow rate of 150 mL / min. After cooling, filter and wash several times with deionized water, and dry them in a 90 °C forced air drying oven for 18 h to obtain nitrogen-doped biochar.

[0055] (3) The nitrogen-doped biochar was added to a pre-prepared nickel nitrate solution (the mass fraction of nickel relative to the nitrogen-doped biochar was 6%) and stirred for 10 minutes. The mixture was ultrasonically impregnated for 40 minutes, and then the impregnated mixture was transferred to an autoclave and heat treated at 300°C for 12 hours. After cooling, the mixture was dried in a 90°C forced air drying oven for 18 hours.

[0056] (4) The solid obtained in step (3) was calcined and reduced in a 100% hydrogen atmosphere (hydrogen flow rate: 50 mL / min) using a tubular furnace (heating rate: 20°C / min) for 1 h to obtain a nitrogen-doped biochar / transition metal catalyst.

[0057] Comparative Example 1

[0058] A method for preparing nitrogen-doped biochar comprises the following steps:

[0059] (1) The discarded wheat straw was crushed and sieved into 60-80 mesh, added into deionized water, stirred and washed for 12 h, dried in a 105 °C forced air drying oven for 12 h, and calcined at 750 °C for 1 h (heating rate: 10 °C / min) under nitrogen gas with a nitrogen flow rate of 50 mL / min to obtain biochar.

[0060] (2) Add 0.2 g of melamine and 4.0 g of potassium hydroxide to 2 g of biochar and grind them thoroughly. Then, calcine them under 10% CO2 gas for 1 h (heating rate: 10°C / min) with a CO2 flow rate of 50 mL / min. After cooling, filter and wash them several times with deionized water, and dry them in a 105°C forced air drying oven for 12 h to obtain nitrogen-doped biochar.

[0061] Comparative Example 2

[0062] A method for preparing biochar comprises the following steps:

[0063] The discarded wheat straw was crushed and sieved into 60-80 mesh, added into deionized water and stirred and washed for 12 h, dried in a 105°C forced air drying oven for 12 h, and calcined at 750°C for 1 h (heating rate: 10°C / min) under nitrogen gas with a nitrogen flow rate of 50 mL / min to obtain biochar.

[0064] Comparative Example 3

[0065] A method for preparing a biomass charcoal / transition metal catalyst comprises the following steps:

[0066] (1) The discarded wheat straw was crushed and sieved into 60-80 mesh, added into deionized water, stirred and washed for 12 h, dried in a 105 °C forced air drying oven for 12 h, and calcined at 750 °C for 1 h (heating rate: 10 °C / min) under nitrogen gas with a nitrogen flow rate of 50 mL / min to obtain biochar.

[0067] (2) Add 2 g of biochar into a pre-prepared nickel nitrate solution (the mass fraction of nickel relative to nitrogen-doped biochar is 5%) and stir for 15 min. Ultrasonic impregnation treatment is performed for 15 min. The impregnated mixture is then transferred to an autoclave and heat treated at 250 °C for 12 h. After cooling, the mixture is dried in a 105 °C forced air drying oven for 24 h.

[0068] (3) The solid obtained in step (3) was calcined and reduced in a 15% hydrogen atmosphere (hydrogen flow rate: 50 mL / min) using a tubular furnace (heating rate: 10°C / min) for 1 h to obtain a biochar / transition metal catalyst.

[0069] Comparative Example 4

[0070] A method for preparing a nitrogen-doped biochar / transition metal catalyst comprises the following steps:

[0071] (1) The discarded wheat straw was crushed and sieved into 60-80 mesh, added into deionized water, stirred and washed for 12 h, dried in a 105 °C forced air drying oven for 12 h, and calcined at 750 °C for 1 h (heating rate: 10 °C / min) under nitrogen gas with a nitrogen flow rate of 50 mL / min to obtain biochar.

[0072] (2) Add 0.2 g of melamine and 4.0 g of potassium hydroxide to 2 g of biochar and grind them thoroughly. Then, calcine them under 10% CO2 gas for 1 h (heating rate: 10°C / min) with a CO2 flow rate of 50 mL / min. After cooling, filter and wash them several times with deionized water, and dry them in a 105°C forced air drying oven for 12 h to obtain nitrogen-doped biochar.

[0073] (3) The nitrogen-doped biochar was added to a pre-prepared nickel nitrate solution (the mass fraction of nickel relative to the nitrogen-doped biochar was 5%) and stirred for 15 minutes, ultrasonically impregnated for 12 hours, and then the mixture was dried in a forced air drying oven at 105°C for 24 hours.

[0074] (4) The solid obtained in step (3) was calcined and reduced in a 15% hydrogen atmosphere (hydrogen flow rate: 50 mL / min) using a tubular furnace (heating rate: 10°C / min) for 1 h to obtain a nitrogen-doped biochar / transition metal catalyst.

[0075] Comparative Example 5

[0076] A method for preparing a nitrogen-doped biochar / transition metal catalyst comprises the following steps:

[0077] (1) The discarded wheat straw was crushed and sieved into 60-80 mesh, added into deionized water, stirred and washed for 12 h, dried in a 105 °C forced air drying oven for 12 h, and calcined at 750 °C for 1 h (heating rate: 10 °C / min) under nitrogen gas with a nitrogen flow rate of 50 mL / min to obtain biochar.

[0078] (2) Add 0.2 g of melamine and 4.0 g of potassium hydroxide to 2 g of biochar and grind them thoroughly. Then, calcine them under nitrogen gas for 1 h (heating rate: 10 °C / min) with a nitrogen flow rate of 50 mL / min. After cooling, filter and wash them several times with deionized water, and dry them in a 105 °C forced air drying oven for 12 h to obtain nitrogen-doped biochar.

[0079] (3) The nitrogen-doped biochar was added to a pre-prepared nickel nitrate solution (the mass fraction of nickel relative to the nitrogen-doped biochar was 5%) and stirred for 15 minutes. The mixture was ultrasonically impregnated for 15 minutes, and then the impregnated mixture was transferred to an autoclave and heat treated at 250°C for 12 hours. After cooling, the mixture was dried in a 105°C forced air drying oven for 24 hours.

[0080] (4) The solid obtained in step (3) was calcined and reduced in a 15% hydrogen atmosphere (hydrogen flow rate: 50 mL / min) using a tubular furnace (heating rate: 10°C / min) for 1 h to obtain a nitrogen-doped biochar / transition metal catalyst.

[0081] Comparative Example 6

[0082] A method for preparing a nitrogen-doped biochar / transition metal catalyst comprises the following steps:

[0083] (1) The waste wheat straw was crushed and sieved into 60-80 mesh, added into deionized water, stirred and washed for 12 h, dried in a 105 °C forced air drying oven for 12 h, added with 0.2 g melamine and 4.0 g potassium hydroxide, and fully ground, and then calcined at 750 °C for 2 h (heating rate: 10 °C / min) under nitrogen gas with a nitrogen flow rate of 50 mL / min to obtain nitrogen-doped biochar.

[0084] (2) The nitrogen-doped biochar was added to a pre-prepared nickel nitrate solution (the mass fraction of nickel relative to the nitrogen-doped biochar was 5%) and stirred for 15 minutes, ultrasonically impregnated for 15 minutes, and then the impregnated mixture was transferred to an autoclave and heat treated at 250°C for 12 hours. After cooling, the mixture was dried in a 105°C forced air drying oven for 24 hours.

[0085] (3) The solid obtained in step (2) was calcined and reduced in a 15% hydrogen atmosphere (hydrogen flow rate: 50 mL / min) using a tubular furnace (heating rate: 10°C / min) for 1 h to obtain a nitrogen-doped biochar / transition metal catalyst.

[0086] Effect example

[0087] The materials prepared in Examples 1-7 and Comparative Examples 1-6 were subjected to catalytic pyrolysis of coal tar in a fast-heating fixed-bed reactor to prepare aromatic hydrocarbons, specifically comprising: 1.0 mg of coal tar (the components of coal tar are shown in Figure 1 ) was added into a quartz tube and a small amount of quartz wool was filled on both sides of the coal tar. 1.5 mg of catalyst was placed on each side of the coal tar. The pyrolysis temperature was set to 500 ° C and the time was 1 min. After pyrolysis, the components of the coal tar were catalytically pyrolyzed by the catalyst bed. The pyrolysis products were analyzed by gas chromatography-mass spectrometry. The relative yield of aromatics and the selectivity of light aromatics are shown in Table 1.

[0088] Relative yield R of organic compounds in pyrolysis products yield Determined by semi-quantitative method of chromatographic peak area percentage:

[0089]

[0090] Where P is the peak area of ​​a specific type of organic compound, P total is the total peak area of ​​all organic compounds.

[0091] Light aromatics (C6-C 10 ) is selectively determined as:

[0092]

[0093] Where S L It is a light aromatic hydrocarbon (C6-C 10) selectivity, R L It is a light aromatic hydrocarbon (C6-C 10 ) relative yield, R a is the relative yield of aromatics.

[0094] Table 1

[0095] Aromatic hydrocarbon yield (%) Light aromatics selectivity (%) Example 1 80.30 91.03 Example 2 83.14 95.06 Example 3 80.12 94.65 Example 4 79.19 95.34 Example 5 81.76 94.83 Example 6 80.82 91.65 Example 7 79.27 89.01 Comparative Example 1 67.27 79.89 Comparative Example 2 47.39 44.04 Comparative Example 3 41.83 41.17 No catalyst 42.27 29.62

[0096] Depend on Figure 1 It can be seen that compared with comparative examples 1-3, the catalysts prepared in Examples 1-7 have higher aromatics yields and light aromatics selectivity. In the nitrogen-doped biochar / transition metal catalyst prepared by the present invention, nitrogen doping improves the defect structure of the catalyst, promotes electron transfer, optimizes the charge distribution of the catalyst, and the transition metal particles are small in size and evenly dispersed, thus having excellent catalytic activity, mild reaction conditions, high light aromatics selectivity, simple process, and suitable for large-scale application.

[0097] The tar was directly pyrolyzed under non-catalytic pyrolysis without catalyst, and the yield of aromatics was only 42.27, and the light aromatics (C6-C 10 ) selectivity is 29.62%.

[0098] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a nitrogen-doped biochar / transition metal catalyst, characterized in that: The steps include: (1) calcining the waste biomass under inert gas to obtain biochar, then adding a nitrogen source and a strong base, mixing evenly, calcining under CO2 gas, and finally washing and drying to obtain nitrogen-doped biochar; (2) Immersing nitrogen-doped biochar in a transition metal salt solution, stirring, and ultrasonicating, and then sequentially performing a hydrothermal reaction, drying, and calcining under hydrogen to obtain a nitrogen-doped carbon / transition metal catalyst.

2. The method for preparing the nitrogen-doped biochar / transition metal catalyst according to claim 1, wherein: The waste biomass is one of wheat straw, tobacco stems, pine needles and corn straw.

3. The method for preparing the nitrogen-doped biochar / transition metal catalyst according to claim 1, wherein: In the step (1), the waste biomass is calcined under inert gas at a temperature of 550-900° C., a time of 1-2 hours, a heating rate of 10-40° C. / min, and a flow rate of the inert gas of 20-150 ml / min.

4. The method for preparing the nitrogen-doped biochar / transition metal catalyst according to claim 1, wherein: In the step (1), the calcination temperature under CO2 gas is 600-900°C, the time is 1-3 hours, the concentration of CO2 is 5% to 100%, and the flow rate is 20 to 150 mL / min.

5. The method for preparing the nitrogen-doped biochar / transition metal catalyst according to claim 1, wherein: The nitrogen source is at least one of melamine, urea, and polyethylene glycol; the strong base is one of sodium hydroxide, potassium hydroxide, and calcium hydroxide; and the mass ratio of the biochar, nitrogen source, and strong base is 2-5:0.2-0.8:1-5.

6. The method for preparing the nitrogen-doped biochar / transition metal catalyst according to claim 1, wherein: The transition metal salt is at least one of nickel nitrate, cobalt nitrate, iron nitrate and copper nitrate, and the mass of the transition metal salt is 1-10% of the mass of the nitrogen-doped biomass carbon.

7. The method for preparing the nitrogen-doped biochar / transition metal catalyst according to claim 1, wherein: In the step (2), the stirring time is 10-30 min, the ultrasonic time is 20-40 min; the temperature of the hydrothermal reaction is 150-300° C., and the time is 12-24 h.

8. The method for preparing the nitrogen-doped biochar / transition metal catalyst according to claim 1, wherein: In the step (2), the calcination temperature under hydrogen is 700-900° C., the calcination time is 30-120 min, the concentration of hydrogen is 3%-100%, and the flow rate is 50-100 mL / min. 9 . The nitrogen-doped biochar / transition metal catalyst prepared by the method for preparing the nitrogen-doped biochar / transition metal catalyst according to claim 1 .

10. Use of the nitrogen-doped biochar / transition metal catalyst according to claim 9 in the preparation of aromatic hydrocarbons by catalytic pyrolysis of coal tar.

Citation Information

Patent Citations

  • Preparing of Ni2P / Zr-MCM-41 catalyst and application for preparing biofuel by catalyzed biolipid

    CN105536860A

  • High-activity hydrodeoxygenation catalyst and preparation method and application thereof

    CN107537477A

  • Preparation method of hierarchical pore carbon-based catalyst for catalytic reforming of coal tar

    CN109529853A

  • Method for preparing furfuryl alcohol by catalyzing transfer hydrogenation of furfural through non-noble metal-loaded nitrogen-doped carbon

    CN111087370A

  • Nickel-loaded nitrogen-doped hierarchical pore biochar material as well as preparation method and application thereof

    CN115212911A