Anion-regulated silicon-based microaggregate negative electrode material and preparation method and use thereof

Through the preparation method of anion-controlled siloxane-based micro-agglomerate negative electrode material, the problems of low sodium storage and poor conductivity of the negative electrode material of sodium ion battery are solved, significantly improving the diffusion performance and sodium storage characteristics of sodium ions/electrons, and improving sodium ions Cycle stability and rate performance of the battery.

CN115172701BActive Publication Date: 2024-11-26NORTHWEST UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210853732.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-12
Publication Date
2024-11-26
Estimated Expiration
2042-07-12

AI Technical Summary

Technical Problem

The low sodium storage amount of sodium ion battery negative electrode materials, large volume effect during charging and discharging, and poor conductivity limit the development of sodium ion batteries, especially due to the slow diffusion of sodium ions in silicon materials.

Method used

Using the preparation method of anion-controlled siloxane-based micro-agglomerate negative electrode material, SiO2@RF suspension is formed by adding resorcinol and formaldehyde to ethyl silicate, and dopamine hydrochloride and pyrrole are added to adjust the pH value to form SiO2@RF/ PDA-PPY microagglomerates are reduced and charred by magnesium thermal reaction, and S, Se or P anions are added to form S-Si@HC/NC microagglomerates to improve the diffusion performance of sodium ions/electrons.

Benefits of technology

It significantly improves the transmission performance of sodium ions/electrons inside the material lattice, enhances the sodium storage characteristics and conductivity, and improves the cycling stability and rate performance of sodium ion batteries, especially at high current density, the sodium storage volume remains good.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115172701B_ABST
    Figure CN115172701B_ABST
Patent Text Reader

Abstract

The present invention relates to a sodium ion battery, and in particular to an anion-regulated silicon-based microaggregate negative electrode material, and a preparation method and use thereof. The preparation of the negative electrode material comprises the following steps: 1. preparing nano-scale SiO2@RF balls; 2. forming SiO2@RF / PDA‑PPY microaggregates; 3. forming Si@HC / NC microaggregates; 4. obtaining the target product X‑Si@HC / NC microaggregates. The electrical performance of the S‑Si@HC / NC microaggregate balls prepared by the present invention is significantly better than that of Si@HC. At a current density of 0.5A / g, after 200 long cycles, the sodium storage capacity of S‑Si@HC / NC can still be maintained at 491mAh / g; at the same time, S‑Si@HC / NC exhibits excellent rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a sodium ion battery, and in particular to an anion-regulated silicon-based microaggregate negative electrode material and a preparation method and use thereof. Background Art

[0002] Sodium-ion battery is a secondary battery (rechargeable battery) that mainly relies on the movement of sodium ions between the positive and negative electrodes to work. The electrode material used in sodium-ion batteries is mainly sodium salt, which is more abundant and cheaper than lithium salt. Since the radius of sodium ions is larger than that of lithium ions, So when weight and energy density are not high requirements, sodium-ion batteries are a cost-effective alternative.

[0003] Compared with lithium-ion batteries, sodium-ion batteries have the following advantages: (1) Sodium salt raw materials are abundant and inexpensive. The use of iron-manganese-nickel-based positive electrode materials reduces the cost of raw materials by half compared to lithium-ion battery ternary positive electrode materials; (2) Due to the characteristics of sodium salt, low-concentration electrolytes can be used (for the same concentration of electrolyte, the conductivity of sodium salt is about 20% higher than that of lithium electrolyte) to reduce costs; (3) Sodium ions do not form alloys with aluminum, and aluminum foil can be used as the negative electrode collector, which can further reduce costs by about 8% and weight by about 10%; (4) Due to the sodium-ion battery's non-overdischarge characteristic, sodium-ion batteries are allowed to discharge to zero volts. The energy density of sodium-ion batteries is greater than 100Wh / kg, which is comparable to lithium iron phosphate batteries, but its cost advantage is obvious, and it is expected to replace traditional lead-acid batteries in large-scale energy storage.

[0004] Although sodium-ion batteries have the advantages of low price and environmental friendliness, which are suitable for large-scale applications, the current research and development of sodium-ion batteries is restricted by factors such as positive and negative electrode materials, binders, diaphragms, electrolytes, and battery assembly technology. Among them, the low sodium storage capacity of the negative electrode materials of sodium-ion batteries, the large volume effect during charging and discharging, and the poor conductivity of the negative electrode materials themselves are the core issues restricting the development of sodium-ion batteries. Among different types of negative electrode materials, alloy silicon has the advantages of high theoretical specific capacity, low working voltage, abundant reserves in nature, and low price, which are suitable for large-scale applications. Silicon can react with sodium to form NaSi, with a theoretical sodium storage capacity of up to 960mAh / g, which is higher than the sodium storage capacity of most alloy materials. At the same time, silicon has achieved great success in scientific research and industrial application as a negative electrode material for lithium-ion batteries, which provides a good research and application foundation for silicon as a negative electrode material for sodium-ion batteries. However, due to the small lattice band gap and atomic gap of silicon, the diffusion of sodium ions / electrons in the silicon lattice is affected, thereby affecting the sodium storage characteristics of silicon negative electrode materials. Summary of the invention

[0005] The purpose of the present invention is to effectively improve the band gap and atomic spacing of the material lattice, enhance the diffusion of sodium ions / electrons in the material lattice, construct a new silicon-carbon composite material to improve the sodium storage characteristics of silicon negative electrode materials, solve the problem of slow sodium ion diffusion of silicon, and thus improve the transmission performance of sodium ions / electrons in the material lattice. Based on this, the present invention proposes a method for preparing anion-regulated silicon-based microaggregate sodium ion battery negative electrode material.

[0006] The method for preparing anion-regulated silicon-based microaggregate sodium ion battery negative electrode material provided by the present invention comprises the following steps:

[0007] Resorcinol and formaldehyde were added to tetraethyl orthosilicate to obtain SiO2@RF suspension;

[0008] The pH of the SiO2@RF suspension is adjusted to alkaline, and dopamine hydrochloride and pyrrole are added to form SiO2@RF / PDA-PPY microaggregates;

[0009] Reducing the silicon dioxide in the SiO2@RF / PDA-PPY microaggregates by magnesium thermal reaction, and carbonizing the resorcinol-formaldehyde and dopamine-modified polypyrrole therein to obtain Si@HC / NC microaggregates;

[0010] The raw material containing S, Se or P anions is mixed with the Si@HC / NC microaggregates, and calcined under an inert environment to obtain the target product S-Si@HC / NC microaggregates.

[0011] Preferably, the usage ratio of the ethyl orthosilicate, the m-diphenol and the formaldehyde is 2-5 ml: 0.1-0.6 g: 0.3-0.7 ml.

[0012] Preferably, the pH of the SiO2@RF suspension is adjusted to be alkaline by adjusting the pH to 9.0 to 11.5;

[0013] The usage ratio of the SiO2@RF suspension, the dopamine hydrochloride and the pyrrole is 10-30 ml: 0.06-0.36 g: 0.2-1 ml.

[0014] Preferably, the specific process of the magnesium thermal reaction is: mixing the SiO2@RF / PDA-PPY microaggregates with magnesium powder, heating the mixture to 600°C to 750°C at a heating rate of 3°C / min to 8°C / min in an inert environment, and reacting the mixture for 1.5 to 4 hours.

[0015] Preferably, the mass ratio of the SiO2@RF / PDA-PPY microaggregates to the magnesium powder is 1:1-3.

[0016] Preferably, the mass ratio of the raw material containing S, Se or P anions to the Si@HC / NC microaggregates is 1:5-10;

[0017] The raw material containing S anions is sulfur powder, the raw material containing Se anions is selenium powder, and the raw material containing P anions is red phosphorus or sodium hypophosphite;

[0018] The calcination is carried out by heating the temperature to 550°C to 750°C at a heating rate of 5°C / min to 10°C / min for 2-8h.

[0019] The present invention also provides an anion-regulated silicon-based microaggregate negative electrode material prepared according to the above method.

[0020] Another object of the present invention is to provide the use of the anion-regulated silicon-based microaggregate negative electrode material in the preparation of a sodium ion battery.

[0021] Another object of the present invention is to provide a negative electrode sheet, comprising:

[0022] a current collector; and

[0023] The membrane is arranged on the current collector and comprises a conductive agent, a binder and the anion-regulated silicon-based microaggregate negative electrode material.

[0024] Another object of the present invention is to provide a sodium ion battery comprising the negative electrode sheet.

[0025] Compared with the prior art, the beneficial effects of the present invention are:

[0026] 1. The present invention adopts traditional external interface regulation methods (such as material nano-sizing, silicon-carbon material composite, construction of hollow structure and micro-aggregate, etc.) and anion doping regulation methods to improve the sodium ion / electron conductivity and composite structure stability of silicon-based composite materials.

[0027] 2. The present invention utilizes S, Se and P anions to regulate and modify silicon materials, which can increase the electron / hole density inside the material to accelerate electron transmission, and the doping-induced deformation can cause barrier fluctuations and silicon lattice changes to provide a lower barrier for a faster sodium ion diffusion path. At the same time, anions are doped into the silicon lattice to replace some silicon atoms, and the silicon crystal spacing will increase, making it easier for sodium ions to transmit between the lattices. Anion regulation can effectively improve the crystal parameters, energy bands, lattice spacing, and charge distribution of nanomaterials, thereby effectively solving the problem of slow sodium ion diffusion in silicon, thereby improving the transmission performance of sodium ions / electrons inside the material lattice.

[0028] 3. The sodium ion battery negative electrode material S-Si@HC / NC prepared by the present invention can maintain a sodium storage capacity of 491mAh / g after 200 long cycles at a current density of 0.5A / g. At the same time, S-Si@HC / NC has good rate performance. At different current densities such as 0.1A / g, 0.2A / g, 0.4A / g, 0.8A / g, 1.6A / g, 3.2A / g and 0.2A / g, S-Si@HC / NC has stable charge and discharge performance. In particular, at a large current of 3.2A / g, the sodium storage capacity can still be as high as 256mAh / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the SEM image of SiO2@RF prepared in Example 1;

[0030] Figure 2 This is the SEM image of Si@HC / NC prepared in Example 1;

[0031] Figure 3 This is the SEM image of the S-Si@HC / NC microaggregates prepared in Example 1;

[0032] Figure 4 TEM image of S-Si@HC / NC microaggregates prepared in Example 1;

[0033] Figure 5 XRD pattern of S-Si@HC / NC microaggregates prepared in Example 1;

[0034] Figure 6 Long cycle test of the battery assembled with S-Si@HC / NC micro-aggregate spheres in Example 12;

[0035] Figure 7 The rate performance test of the battery assembled with S-Si@HC / NC micro-aggregate spheres in Example 12;

[0036] Figure 8 This is the SEM image of Si@HC prepared in Comparative Example 1;

[0037] Fig. 9 TEM image of Si@HC prepared in Comparative Example 1;

[0038] Fig.10 XRD pattern of Si@HC prepared in Comparative Example 1;

[0039] Fig.11 This is the long cycle test of Si@HC in Comparative Example 2;

[0040] Fig.12 This is the rate performance test of Si@HC in Comparative Example 2. DETAILED DESCRIPTION

[0041] The present invention is further described in detail below in conjunction with the accompanying drawings and specific examples, but it should not be construed as limiting the present invention. Without departing from the spirit and substance of the present invention, the modification or replacement of the method, steps or conditions of the present invention all belong to the scope of the present invention. The experimental methods and reagents without specifying the specific conditions in the examples are all in accordance with the conventional conditions in the art.

[0042] Example 1

[0043] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is completed by the following steps:

[0044] 1. Preparation of nano-scale SiO2@RF spheres;

[0045] First, 50 mL of anhydrous ethanol, 7 mL of deionized water, and 1.5 mL of ammonia water were mixed under vigorous stirring to obtain a dispersion, 2 mL of ethyl orthosilicate was slowly added to the dispersion, and then 0.1 g of m-phenol and 0.30 ml of formaldehyde were added, and stirred at 100 r / min at room temperature for 12 h to produce a red SiO2@RF suspension;

[0046] 2. Preparation of SiO2@RF / PDA-PPY microaggregates;

[0047] Take 10 mL of the above SiO2@RF suspension, adjust the pH of the SiO2@RF suspension to 9.0 with 1 mol / L sodium hydroxide solution, add 3 ml of 0.02 g / ml dopamine hydrochloride (DA-HCl) solution and 0.2 ml of pyrrole (PY) to the SiO2@RF suspension, and let it stand for 8 h to form SiO2@RF / PDA-PPY microaggregates;

[0048] 3. Formation of Si@HC / NC microaggregates;

[0049] ① The prepared SiO2@RF / PDA-PPY microaggregates and magnesium powder were mixed in a mass ratio of 1:1 and placed in a quartz boat. The quartz boat was then placed in the middle of a tube furnace. The temperature was raised from room temperature to 600°C at a rate of 3°C / min under argon protection. The silicon dioxide was reduced by magnesium thermal reaction at high temperature for 4 h, and (resorcinol-formaldehyde) RF and (dopamine-modified polypyrrole) PDA-PPY were carbonized at the same time to obtain product 1.

[0050] ② The obtained product 1 was washed with a 15% HCl solution and a 3% HF solution, then allowed to stand for 2 hours and dried for 12 hours to obtain Si@HC / NC microaggregates;

[0051] 4. Preparation of target product X-Si@HC / NC microaggregates;

[0052] The sulfur powder was mixed with the Si@HC / NC microaggregates obtained above at a mass ratio of 1:5, and the mixture was heated to 550°C at a rate of 5°C / min and calcined for 8 h under argon protection to obtain the target product X-Si@HC / NC microaggregates.

[0053] Figure 1 This is the SEM image of SiO2@RF prepared in step 1. Figure 1 It can be seen that SiO2@RF has a uniform spherical shape with a size of 200-300nm.

[0054] Figure 2 This is the SEM image of Si@HC / NC prepared in step 3. Figure 2 It can be seen that SiO2@RF aggregates to form spherical agglomerates with a spherical size of about 1 μm.

[0055] Figure 3 This is the SEM image of the S-Si@HC / NC microaggregates prepared in step 4. Figure 3 It can be seen that the size and morphology of the aggregated spheres have not changed, but S is doped into Si.

[0056] Figure 4 TEM image of S-Si@HC / NC microaggregates prepared in step four. Figure 4 It is proved that nanoparticle S-Si exists in porous hollow carbon.

[0057] Figure 5 This is the XRD pattern of S-Si@HC / NC microaggregates prepared in step 4. Figure 5 It can be seen that S-Si@HC / NC has the lattice of silicon, but due to the doping of S, the crystallinity of Si is lower.

[0058] Example 2

[0059] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is different from that of Example 1 in that 5 mL of ethyl orthosilicate, 0.6 g of m-phenol and 0.70 ml of formaldehyde are added in step 1.

[0060] Example 3

[0061] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is different from that of Example 1 in that in step 2, 6 ml of dopamine hydrochloride (DA-HCl) solution with a mass concentration of 0.06 g / ml and 1.0 ml of pyrrole (PY) are added to the SiO2@RF suspension.

[0062] Example 4

[0063] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is different from Example 1 in that the pH of the SiO2@RF suspension is adjusted to 11.5.

[0064] Example 5

[0065] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is different from that of Example 1 in that in step three, SiO2@RF / PDA-PPY microaggregates and magnesium powder are mixed in a mass ratio of 1:3, and the temperature is raised to 750°C at 8°C / min for reaction for 1.5h.

[0066] Example 6

[0067] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is different from that of Example 1 in that sulfur powder is replaced by selenium powder in step 4.

[0068] Example 7

[0069] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is different from that of Example 1 in that the calcination is carried out under argon protection at a heating rate of 10°C / min to 750°C for 2h.

[0070] Example 8

[0071] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is different from that of Example 1 in that the stirring time in step 1 is 36 hours and the stirring rate is 300 r / min.

[0072] Example 9

[0073] A method for preparing an X-Si@HC / NC microaggregate negative electrode material, which is different from that of Example 1 in that the standing time in step 2 is 24 hours.

[0074] Example 10

[0075] A method for preparing an X-Si@HC / NC microaggregate negative electrode material, which is different from that in Example 1 in that the drying time in step 3② is 24 hours.

[0076] Embodiment 11

[0077] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is different from that of Example 1 in that sulfur powder is replaced by red phosphorus in step 4.

[0078] Example 12

[0079] A method for preparing an X-Si@HC / NC microaggregate negative electrode material is different from that of Example 1 in that in step 4, sulfur powder and Si@HC / NC microaggregates are mixed at a mass ratio of 1:10.

[0080] Embodiment 13

[0081] A CR2025 button-type sodium ion battery is prepared according to the following steps:

[0082] 1. The X-Si@HC / NC microaggregate negative electrode material prepared in Example 1 (the properties of the negative electrode materials prepared in Examples 1 to 12 are substantially the same, so only the negative electrode material prepared in Example 1 is used as an example for description herein) is mixed with acetylene black and a polytetrafluoroethylene aqueous dispersion having a mass fraction of 5% in a mass ratio of 7:2:1 to obtain a mixed slurry;

[0083] 2. adding N-methylpyrrolidone dropwise to the mixed slurry to obtain a mixture for coating;

[0084] The dosage ratio of N-methylpyrrolidone to X-Si@HC / NC microaggregates is 1mL:10mg;

[0085] 3. The coating mixture is evenly coated on an aluminum foil with a diameter of 12 mm, and then vacuum dried at a temperature of 60°C to 80°C for 12h to 18h to obtain an electrode with active substances on the surface, and the mass of the active substances on the electrode is obtained by the difference method;

[0086] The electrode piece containing active substances on the surface is transferred to a vacuum glove box to complete the assembly of the button battery, wherein the polypropylene polymer film is a battery separator, the sodium sheet is a battery counter electrode, and the electrode piece containing active substances on the surface is a working electrode. After the working electrode, the gasket, the separator, the counter electrode and the battery shell are assembled into a CR 2025 button battery in the glove box, the button battery is sealed using a sealing machine, and finally the prepared button battery is left to stand at room temperature for 8 hours to activate the battery, and the gasket is stainless steel; that is, the preparation of the CR 2025 button-type sodium ion battery is completed.

[0087] Figure 6 This is a long cycle test of the battery assembled with S-Si@HC / NC micro-aggregate spheres in Example 12. Figure 6 It can be seen that at a current density of 0.5A / g, after 200 long cycles, the sodium storage capacity of S-Si@HC / NC can still be maintained at 491mAh / g. At the same time, S-Si@HC / NC has good rate performance.

[0088] Figure 7 This is the rate performance test of the battery assembled with S-Si@HC / NC micro-aggregate spheres in Example 12. Figure 7It can be seen that S-Si@HC / NC has stable charge and discharge performance at different current densities such as 0.1A / g, 0.2A / g, 0.4A / g, 0.8A / g, 1.6A / g, 3.2A / g and 0.2A / g. In particular, at a high current of 3.2A / g, the sodium storage capacity can still be as high as 256mAh / g.

[0089] Comparative Example 1

[0090] A method for designing and preparing Si@HC nanoparticles is completed in the following steps:

[0091] 1. Preparation of nano-scale SiO2@RF balls:

[0092] First, 50 mL of anhydrous ethanol, 7 mL of deionized water, and 1.5 mL of ammonia water were mixed under vigorous stirring to obtain a dispersion, 2 mL of ethyl orthosilicate was slowly added to the dispersion, and then 0.1 g of m-phenol and 0.30 ml of formaldehyde were added, and stirred at 100 r / min at room temperature for 12 h to produce a red SiO2@RF suspension;

[0093] 2. Preparation of Si@HC nanoparticles:

[0094] ① The prepared micro-aggregates and magnesium powder were mixed in a mass ratio of 1:3, placed in a quartz boat, and then the quartz boat was placed in the middle of a tube furnace. Under argon protection, the temperature was raised from room temperature to 600°C at a heating rate of 8°C / min, and silicon dioxide was reduced by magnesium thermal reaction at high temperature for 4 hours;

[0095] ② The product obtained in step ① was washed with a 15% HCl solution and a 3% HF solution, left to stand for 2 hours, and dried for 12 hours, thereby obtaining Si@HC nanoparticles.

[0096] Figure 8 This is the SEM image of Si@HC prepared in Comparative Example 1. Figure 8 It can be seen that Si@HC has a uniform spherical shape and the size is between 200-300nm.

[0097] Fig. 9 TEM image of Si@HC prepared in Comparative Example 1. Fig. 9 It can be seen that silicon particles are distributed in the porous hollow carbon.

[0098] Fig.10 XRD pattern of Si@HC prepared in Comparative Example 1. Fig.10 It can be seen that the silicon particles have good crystallinity.

[0099] Comparative Example 2

[0100] A CR2025 button-type sodium ion battery is prepared according to the following steps:

[0101] 1. The Si@HC nanoparticle secondary battery negative electrode material prepared in Comparative Example 1, acetylene black and 5% polytetrafluoroethylene aqueous dispersion emulsion were mixed in a mass ratio of 7:2:1 to obtain a mixed slurry;

[0102] 2. adding N-methylpyrrolidone dropwise to the mixed slurry to obtain a mixture for coating;

[0103] The volume ratio of N-methylpyrrolidone to the mass ratio of the secondary battery negative electrode material of Si@HC nanoparticles was 1 mL: 10 mg;

[0104] 3. The coating mixture is evenly coated on an aluminum foil with a diameter of 12 mm, and then vacuum dried at a temperature of 80°C for 12 hours to obtain a pole piece with an active substance on the surface, and the mass of the active substance on the pole piece is obtained by the difference method; the pole piece with the active substance on the surface is transferred to a vacuum glove box to complete the assembly of the button battery, wherein the polypropylene polymer film is a battery separator, the sodium sheet is a battery counter electrode, and the pole piece with the active substance on the surface is a working electrode. After the working electrode, gasket, diaphragm, counter electrode and battery shell are assembled into a CR 2025 button battery in the glove box, the button battery is sealed with a sealing machine, and finally the prepared button battery is left to stand at room temperature for 8 hours to activate the battery, and the gasket is stainless steel; that is, the preparation of the CR2025 button-type sodium ion battery is completed.

[0105] Fig.11 This is the long cycle test of Si@HC in Comparative Example 2. Fig.11 It can be seen that at a current density of 0.5A / g, after 200 long cycles, the sodium storage capacity of Si@HC is 178mAh / g.

[0106] Fig.12 This is the rate performance test of Si@HC in Comparative Example 2. Fig.12 It can be seen that the charge and discharge performance of Si@HC is relatively poor at different current densities such as 0.1A / g, 0.2A / g, 0.4A / g, 0.8A / g, 1.6A / g, 3.2A / g and 0.2A / g. At a high current of 3.2A / g, the sodium storage capacity is only 54mAh / g.

[0107] The above disclosure is only a specific embodiment of the present invention, but the embodiments of the present invention are not limited thereto, and any changes that can be conceived by those skilled in the art should fall within the protection scope of the present invention.

Claims

1. A method for preparing anion-regulated silicon-based microaggregate negative electrode material, characterized in that: The following steps are involved: Resorcinol and formaldehyde were added to tetraethyl orthosilicate to obtain SiO2@RF suspension; The pH of the SiO2@RF suspension is adjusted to alkaline, and dopamine hydrochloride and pyrrole are added to form SiO2@RF / PDA-PPY microaggregates; Reducing the silicon dioxide in the SiO2@RF / PDA-PPY microaggregates by magnesium thermal reaction, and carbonizing the resorcinol-formaldehyde and dopamine-modified polypyrrole therein to obtain Si@HC / NC microaggregates; Mixing a raw material containing S, Se or P anions with the Si@HC / NC microaggregates, and calcining them under an inert environment to obtain the target product anion-regulated silicon-based microaggregates; Wherein, the usage ratio of the ethyl orthosilicate, the resorcinol and the formaldehyde is 2-5 ml: 0.1-0.6 g: 0.3-0.7 ml; The pH of the SiO2@RF suspension is adjusted to alkaline to 9.0-11.5; the dosage ratio of the SiO2@RF suspension, the dopamine hydrochloride and the pyrrole is 10-30 ml: 0.06-0.36 g: 0.2-1 ml; The specific process of the magnesium thermal reaction is: mixing the SiO2@RF / PDA-PPY microaggregates with magnesium powder, heating to 600°C to 750°C in an inert environment at a heating rate of 3°C / min to 8°C / min for reaction for 1.5 to 4 hours; the mass ratio of the SiO2@RF / PDA-PPY microaggregates to the magnesium powder is 1:1 to 3; The mass ratio of the raw material containing S, Se or P anions to the Si@HC / NC microaggregates is 1:5-10; The raw material containing S anions is sulfur powder, the raw material containing Se anions is selenium powder, and the raw material containing P anions is red phosphorus or sodium hypophosphite; The calcination is carried out at a heating rate of 5°C / min to 10°C / min and the temperature is raised to 550°C to 750°C for 2-8h.

2. An anion-regulated silicon-based microaggregate negative electrode material prepared according to the method of claim 1.

3. Use of the anion-regulated silicon-based microaggregate negative electrode material according to claim 1 in the preparation of sodium ion batteries.

4. A negative electrode sheet, characterized in that: include: current collector; and The membrane is arranged on the current collector and comprises a conductive agent, a binder and the anion-regulated silicon-based microaggregate negative electrode material according to claim 2.

5. A sodium ion battery, characterized in that: Including the negative electrode sheet as claimed in claim 4.

Citation Information

Patent Citations

  • Silicon-containing composite material and its preparation method and application

    CN101210119A

  • Hollow silicon-based composite material, preparation method and lithium ion battery comprising composite material

    CN106129411A

  • A boron doping modified hard carbon coating negative electrode material with high rate performance and a liquid phase preparation method thereof

    CN109148847A

  • A hollow structure silicon-carbon composite material prepared by a magnesium thermal reduction method and a preparation method thereof

    CN109244399A

  • Multi-heteroatom co-doped carbon shell coated silicon composite material and preparation method thereof

    CN111682173A