Green catalyst for degrading low-density polyethylene and preparation method thereof
Through catalytic cracking of solid acid catalysts, a green catalyst is prepared, which solves the complex problems of landfill pollution and thermal cracking products in plastic waste recycling, and achieves high-efficiency green degradation of low-density polyethylene, reduces temperature and energy consumption, and has significant economic and social benefits.
Patent Information
- Application Number
- CN202411073426.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
The existing plastic waste recycling methods have problems such as landfill pollution, complex thermal cracking products, low value, and waste of energy, making it difficult to effectively deal with low-density polyethylene waste.
A solid acid catalyst is used for catalytic cracking, and a green catalyst is prepared by hydrothermal synthesis to reduce the cracking temperature, and the product composition is changed by changing the acidic center strength and pore size of the catalyst to achieve green degradation of low-density polyethylene.
Effectively degrading low-density polyethylene reduces cracking temperature and energy efficiency, simplifies processes, reduces equipment investment and energy consumption, and has important economic and social benefits.
Smart Images

Figure CN118976531A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and specifically discloses a catalyst for green degradation of low-density polyethylene and a preparation method thereof. Background Art
[0002] Over the past century, plastics have been widely used in packaging, manufacturing, agriculture and other fields due to their excellent performance and good chemical stability. The global production and use of plastics have increased year by year, but the treatment of waste plastics is still very limited. Every year, 300 million tons of waste plastics are generated worldwide, of which only 9% are recycled, 12% are incinerated, and 79% are landfilled or abandoned in nature, causing irreversible damage to the global ecosystem and human health.
[0003] Despite the emergence of policies requiring recycling and higher levels of resource conservation, landfilling remains the preferred method for disposing plastic waste. However, this option brings with it various constraints, involving the volume occupied by plastic relative to its weight and the loss of natural resources represented by this practice. Another option is material recycling, in which plastics are re-granulated and reused, but it is limited by the necessity to collect pure and high-quality plastics, as well as the market for the products. Therefore, raw material recovery of plastic waste has become a reliable option for converting plastic residues into useful materials. The simplest method for recycling plastic raw materials is thermal cracking, which produces a complex mixture of products with low value as raw chemicals and is mainly used as fuel. However, by converting waste plastics into fuel oil or chemical raw materials through plastic cracking on solid acid catalysts, it can not only alleviate resource shortages, but also will not cause secondary pollution to the environment. It is possible to obtain products with higher commercial value and more applications, which is the best choice for the reduction and resource utilization of waste plastics.
[0004] The purpose of the present invention is to provide a green catalyst for degrading low-density polyethylene and a preparation method thereof. Compared with other methods for degrading low-density polyethylene, the catalyst is green and effective and can reduce the cracking reaction temperature and cracking energy efficiency. The composition of the product can be changed by changing the strength of the acid center of the catalyst and the pore size. Summary of the invention
[0005] The purpose of the present invention is to break the limitation of traditional plastic waste recycling methods, and use solid acid catalysts for catalytic cracking, which can not only solve the problem of landfill recycling of plastic waste and pollute the environment, but also solve the problems of complex thermal cracking recycling products, low recycling value, and energy waste. The present invention innovatively develops a green catalyst that can achieve green and effective degradation of low-density polyethylene.
[0006] In a first aspect, the present invention provides a method for preparing a catalyst for green degradation of low-density polyethylene, which specifically comprises the following steps:
[0007] S1: Weigh sodium hydroxide and sodium aluminate separately into the template and stir until completely dissolved;
[0008] The type of the template is tetraethylammonium hydroxide;
[0009] The sodium aluminate is 1 part by mass;
[0010] The amount of sodium hydroxide added is such that the pH value of the system is in the range of 10 to 12;
[0011] The addition amount of the template is 50 to 150 parts by weight;
[0012] S2: Weigh 10-70 parts by mass of silicon dioxide, stir and mix with the solution obtained in step S1, and perform a hydrothermal synthesis reaction at 130° C. to 150° C.;
[0013] The silicon dioxide is fumed silicon dioxide;
[0014] S3: After the hydrothermal reaction in step S2 is completed, the sample is taken out, centrifuged, dried, ground into powder, and calcined at 400-600° C. for 4-8 hours. The calcined product is a catalyst.
[0015] Preferably, in step S1, the pH value is 11.
[0016] Preferably, the hydrothermal reaction time in step S2 is 5 to 7 days.
[0017] Furthermore, the particle size of the fumed silica is 30 to 50 nm.
[0018] Preferably, in step S3, the drying temperature is 60° C., the roasting temperature is 500° C., and the roasting time is 6 hours.
[0019] Preferably, in step S1, the pH value of the synthesis system is 11; in step S2, the amount of silicon dioxide added is such that the molar ratio of silicon to aluminum elements in the system is 50:1, the reaction time is 7 days, and the reaction temperature is 140°C; in step S3, the drying temperature is 60°C; the calcination temperature is 500°C, and the calcination time is 6 hours.
[0020] In a second aspect, the present invention provides a catalyst for green degradation of low-density polyethylene, which is synthesized using the method described in the first aspect.
[0021] In a third aspect, the present invention provides a use of the catalyst described in the second aspect for degrading low-density polyethylene.
[0022] Preferably, the application of degrading low-density polyethylene specifically comprises the following steps: after mixing the catalyst with low-density polyethylene, heating the mixture to not less than 600° C. in an inert gas atmosphere for degradation.
[0023] Furthermore, the catalyst and the low-density polyethylene are mixed in a mass mixing ratio of not less than 1:9.
[0024] The beneficial effects expected to be achieved by the present invention are:
[0025] The green catalyst applied for in the present invention can effectively degrade low-density polyethylene, reduce the cracking temperature, has a simple process, low equipment investment and energy consumption, and has important economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The X-ray powder diffraction pattern of the catalyst prepared in the present invention.
[0027] Figure 2 This is a scanning electron microscope image of the catalyst prepared in the present invention.
[0028] (a) 2μm (b) 500nm;
[0029] Figure 3 This is the nitrogen adsorption diagram of the catalyst prepared in the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the following examples. It should be noted that the present invention is not limited to the following examples.
[0031] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0032] The low-density polyethylene used in the following examples is from the same batch, model LD165.
[0033] Example 1
[0034] This example investigates the preparation and effect of catalysts with different hydrothermal reaction times:
[0035] Weigh 0.04g of sodium hydroxide and 0.0492g of sodium aluminate respectively into 5g of template agent tetraethylammonium hydroxide, and stir until completely dissolved;
[0036] 1.8 g of silicon dioxide was weighed into a reaction kettle so that the molar ratio of silicon to aluminum in the reaction system was 50:1, and the above solution was stirred and mixed, and the mixture was placed in an oven for hydrothermal synthesis at 140° C. for 5 days, 6 days, and 7 days respectively;
[0037] After the hydrothermal reaction is completed, the sample is taken out, centrifuged, dried, ground into powder, and calcined in a muffle furnace. The calcined product is the prepared catalyst.
[0038] In this experiment, a thermogravimetric analyzer was used to study the catalytic performance of the catalyst prepared in the above experiment. The prepared catalyst experimental sample was mixed and ground evenly with low-density polyethylene at a mass mixing ratio of 1:9. About 10 mg of the ground mixed sample was weighed and placed in the crucible of the thermogravimetric analyzer. The N2 flow rate was controlled to 30 mL / min, and the temperature was heated from room temperature (10°C) to 700°C at a heating rate of 10°C / min. The weight loss signal was recorded, and the catalytic cracking rate was evaluated based on the slope of the weight loss curve.
[0039] Table 1 Effect of catalyst degradation of low density polyethylene in Example 1
[0040]
[0041]
[0042] Example 2
[0043] This example investigates the catalyst preparation and effects of the synthesis system with different pH values:
[0044] Weigh three portions of 0.032g, 0.039g, and 0.045g of sodium hydroxide respectively, so that the pH values in the system are 10.5, 11, and 11.5 respectively; weigh three portions of 0.0492g of sodium aluminate respectively in 5g of the template agent tetraethylammonium hydroxide, and stir until completely dissolved;
[0045] Weigh three portions of 1.8 g of silicon dioxide into a reaction kettle so that the molar ratio of silicon to aluminum in the reaction system is 50:1, stir and mix with the above solution, put into an oven, and perform hydrothermal synthesis reaction at 140° C. for 7 days respectively;
[0046] After the hydrothermal reaction is completed, the sample is taken out, centrifuged, dried, ground into powder, and calcined in a muffle furnace. The calcined product is the prepared catalyst; the drying temperature is 60°C; the calcination temperature is 500°C, and the calcination time is 6 hours.
[0047] In this experiment, a thermogravimetric analyzer was used to study the catalytic performance of the catalyst prepared in the above experiment. The prepared catalyst experimental sample was mixed and ground evenly with low-density polyethylene at a mass mixing ratio of 1:9. 10 mg of the ground mixed sample was weighed and placed in the crucible of the thermogravimetric analyzer. The N2 flow rate was controlled to 30 mL / min, and the temperature was heated from room temperature (10°C) to 700°C at a heating rate of 10°C / min. The weight loss signal was recorded, and the catalytic cracking rate was evaluated based on the slope of the weight loss curve.
[0048] Table 2 Effect of catalyst degradation of low density polyethylene in Example 2
[0049] pH value of reaction system 10.5 11 11.5 Catalyst crystallization rate / % 34% 92% 62% Slope of weight loss curve -1.62 -1 -1.46 The fastest degradation rate corresponds to the temperature / ℃ 453 392 435
[0050] Example 3
[0051] Preparation of catalysts with different silicon-aluminum ratios:
[0052] Weigh 0.04g of sodium hydroxide and 0.0492g of sodium aluminate respectively into 5g of template agent tetraethylammonium hydroxide, and stir until completely dissolved;
[0053] 0.36 g, 1.8 g, and 2.52 g of silicon dioxide were weighed into a reaction kettle respectively, so that the molar ratio of silicon to aluminum in the reaction system was 10:1, 50:1, and 70:1, and the above solution was stirred and mixed, and the mixture was placed in an oven for hydrothermal synthesis reaction at 140° C. for 7 days respectively;
[0054] After the hydrothermal reaction is completed, the sample is taken out, centrifuged, dried, ground into powder, and calcined in a muffle furnace. The calcined product is the prepared catalyst; the drying temperature is 60°C; the calcination temperature is 500°C, and the calcination time is 6 hours.
[0055] The catalytic performance of the catalyst prepared in the above experiment was studied using a thermogravimetric analyzer. The prepared catalyst experimental sample was mixed and ground evenly with low-density polyethylene at a mass mixing ratio of 1:9. About 10 mg of the ground mixed sample was weighed and placed in the crucible of the thermogravimetric analyzer, the N2 flow rate was controlled to 30 mL / min, and the temperature was heated from room temperature (10°C) to 700°C at a heating rate of 10°C / min, and the weight loss signal was recorded. The catalytic cracking rate was evaluated based on the slope of the weight loss curve.
[0056] Table 3 Effect of catalyst degradation of low density polyethylene in Example 3
[0057] Catalyst Si / Al ratio No 10 50 70 Catalyst crystallization rate / % / 90% 92% 89% Slope of weight loss curve -1.72 -1.23 -1 -1.32 The fastest degradation rate corresponds to the temperature / ℃ 464 405 392 419
[0058] Example 4
[0059] Preparation of catalysts at different reaction temperatures:
[0060] Weigh 0.04g of sodium hydroxide and 0.0492g of sodium aluminate respectively into 5g of template agent tetraethylammonium hydroxide, and stir until completely dissolved;
[0061] Weigh 1.8g of silicon dioxide into the reaction kettle, so that the molar ratio of silicon to aluminum in the reaction system is 50:1, and stir and mix with the above solution, and put it into the oven. Perform hydrothermal synthesis reaction at 130℃, 140℃, and 150℃ for 7 days;
[0062] After the hydrothermal reaction is completed, the sample is taken out, centrifuged, dried, ground into powder, and calcined in a muffle furnace. The calcined product is the prepared catalyst; the drying temperature is 60°C; the calcination temperature is 500°C, and the calcination time is 6 hours.
[0063] The catalytic performance of the catalyst prepared in the above experiment was studied using a thermogravimetric analyzer. The prepared catalyst experimental sample was mixed and ground evenly with low-density polyethylene at a mass mixing ratio of 1:9. About 10 mg of the ground mixed sample was weighed and placed in the crucible of the thermogravimetric analyzer, the N2 flow rate was controlled to 30 mL / min, and the temperature was heated from room temperature (10°C) to 700°C at a heating rate of 10°C / min, and the weight loss signal was recorded. The catalytic cracking rate was evaluated based on the slope of the weight loss curve.
[0064] Table 4 Effect of catalyst degradation of low density polyethylene in Example 4
[0065] Hydrothermal reaction temperature / ℃ 130 140 150 Catalyst crystallization rate / % 36% 92% 83% Slope of weight loss curve -1.58 -1 -1.34 The fastest degradation rate corresponds to the temperature / ℃ 450 392 426
[0066] Test results
[0067] Without adding a catalyst to crack low-density polyethylene, the fastest degradation rate corresponds to a temperature of 464°C, and the slope of the weight loss curve is -1.72. Compared with cracking low-density polyethylene without adding a catalyst, the catalysts prepared according to the methods of Examples 1, 2, 3, and 4 have a low degradation temperature and a fast degradation rate in terms of catalytic effect. From the above test results, it can be seen that the catalysts prepared by the methods of Examples 1, 2, 3, and 4 are used to degrade low-density polyethylene, and the effect is good, and it can be degraded greenly and effectively.
[0068] When the catalyst formula silicon-aluminum ratio is 50, the reaction time is 7 days, the reaction temperature is 140°C, and the pH value of the synthesis system is 11, the prepared aluminosilicate catalyst has a high cracking temperature reduction, a fast degradation rate, and a good catalytic effect. The performance characteristics of the catalyst prepared under these conditions are as follows Figure 1 , Figure 2 , Figure 3 shown.
[0069] Figure 1The X-ray powder diffraction diagram of the prepared catalyst shows that, under the optimal formulation conditions, the obtained catalyst has a higher crystallinity.
[0070] Figure 2 This is a scanning electron microscope image of the prepared catalyst. It can be seen from the image that under the optimal formulation conditions, the catalyst has a regular morphology, a particle size at the nanometer level, and a high degree of crystallinity.
[0071] Figure 3 This is the nitrogen adsorption diagram of the prepared catalyst. It can be seen from the figure that under the optimal formulation conditions, the catalyst has a multi-level pore structure and a large specific surface area. The open specific surface area provides abundant active sites for the catalytic reaction and has excellent catalytic performance.
Claims
1. A method for preparing a catalyst for green degradation of low-density polyethylene, characterized in that: The specific steps include: S1: Weigh sodium hydroxide and sodium aluminate separately into the template and stir until completely dissolved; The template agent is tetraethylammonium hydroxide; The sodium aluminate is 1 part by mass; The amount of sodium hydroxide added is such that the pH value of the system is in the range of 10 to 12; The addition amount of the template agent is 50 to 150 parts by weight; S2: Weigh 10 to 70 parts by mass of silicon dioxide, stir and mix with the solution obtained in step S1, and perform a hydrothermal synthesis reaction at 130° C. to 150° C.; S3: After the hydrothermal reaction in step S2 is completed, the sample is taken out, centrifuged, dried, ground into powder, and calcined at 400-600° C. for 4-8 hours. The calcined product is a catalyst.
2. The method for preparing a green catalyst for degrading low-density polyethylene according to claim 1, characterized in that: In step S1, the pH value is 11.
3. The method for preparing a catalyst for green degradation of low-density polyethylene according to claim 1, characterized in that: The hydrothermal reaction time in step S2 is 5 to 7 days.
4. The method for preparing a green catalyst for degrading low-density polyethylene according to claim 1, characterized in that: The particle size of the fumed silica is 30 to 50 nm.
5. The method for preparing a green catalyst for degrading low-density polyethylene according to claim 1, characterized in that: In step S3, the drying temperature is 60° C., the roasting temperature is 500° C., and the roasting time is 6 hours.
6. The method for preparing a green catalyst for degrading low-density polyethylene according to claim 1, characterized in that: The pH value of the synthesis system in step S1 is 11; the amount of silicon dioxide added in step S2 is such that the molar ratio of silicon to aluminum elements in the system is 50:1, the reaction time is 7 days, and the reaction temperature is 140°C; the drying temperature in step S3 is 60°C; the roasting temperature is 500°C, and the roasting time is 6 hours.
7. A green catalyst for degrading low-density polyethylene synthesized by the method described in any one of claims 1 to 6.
8. Use of the catalyst according to claim 7 for degrading low-density polyethylene.
9. Use of the catalyst according to claim 7 for degrading low-density polyethylene, characterized in that: The application of degrading low-density polyethylene specifically comprises the following steps: after mixing the catalyst with low-density polyethylene, heating the mixture to not less than 600° C. in an inert gas atmosphere for degradation.
10. Use of the catalyst according to claim 9 for degrading low-density polyethylene, characterized in that: The catalyst and low-density polyethylene are mixed in a mass ratio of not less than 1:9.
Citation Information
Patent Citations
HMS@NiPt@Beta core-shell structure catalytic material and preparation method and application thereof