UiO-66 (Zr / Hf)-based adsorption material for photocatalysis as well as preparation method and application of UiO-66 (Zr / Hf)-based adsorption material

By replacing Zr4+ with Hf4+ in UiO-66, UiO-66 (Zr/Hf)-based adsorbent material is formed, the problems of low efficiency and insufficient stability of photocatalysts are solved, and efficient degradation and stability of organic pollutants in water are achieved. promote.

CN118976538APending Publication Date: 2024-11-19ZHENJIANG COLLEGE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411045171.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing photocatalysts generate electron holes quickly under light induction, resulting in low photocatalytic efficiency, and the electron transfer efficiency and pore mass transfer process of MOFs materials limit their photocatalytic activity.

Method used

By partially replacing Zr4+ to Hf4+ in UiO-66, UiO-66 (Zr/Hf)-based adsorption material is formed, the energy gap bandwidth is reduced, electrons are promoted from ligand to Zr4+ active site, and the photocatalytic degradation performance of the catalyst is enhanced.

Benefits of technology

The adsorption capacity and catalytic activity of photocatalytic degraded materials are significantly improved, and the degradation rate of organic matter by 4~11% compared with other catalysts is increased, and the thermal and chemical stability of the materials are maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976538A_ABST
    Figure CN118976538A_ABST
Patent Text Reader

Abstract

The invention relates to a UiO-66 (Zr / Hf)-based adsorbing material for photocatalytic degradation of organic pollutants in water as well as a preparation method and application of the material. The preparation method comprises the following steps: S1, adding an organic ligand and zirconium chloride into a DMF (Dimethyl Formamide) solvent, adding acetic acid, and carrying out hydrothermal reaction to obtain a UiO-66-based material; s2, dispersing hafnium chloride in anhydrous dichloroethane, then adding THF and normal hexane, reacting at 0 DEG C under the protection of N2 to obtain a yellow precipitate HfCl4 (THF) 2, filtering, washing and drying; and S3, mixing the UiO-66-based material, HfCl4 (THF) 2 and DMF, carrying out a reaction at 120 DEG C for 5-20 h, washing a solid product, and carrying out vacuum drying to obtain the UiO-66 (Zr / Hf)-based material. The photocatalytic degradation material can be used for photocatalytic degradation of organic pollutants in water, and the adsorption capacity and catalytic activity of the photocatalytic degradation material can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a UiO-66 (Zr / Hf)-based adsorption material for photocatalytic degradation of organic pollutants in water, and a preparation method and application of the material. Background Art

[0002] The search for green and effective ways to degrade pollutants in water has become a current research hotspot. Degrading organic pollutants through semiconductor-based photocatalysts is considered to be an efficient and environmentally friendly method. However, due to the photoinduced electron-hole pairs - -h + The rapid generation of MOFs often leads to low photocatalytic efficiency. Studies have found that the above problem can be solved by combining with other noble metals. It is reported that heterojunction photocatalysts prepared with two semiconductor materials with suitable energy bands can significantly improve the photocatalytic performance. However, the activity and stability of these materials still need to be further improved to meet the needs of practical applications. Metal-organic framework materials (MOFs) are porous materials formed by metal clusters interconnected by organic ligands. Due to their advantages such as high specific surface area, adjustable pore size and functionalization, they have attracted widespread attention in many fields. In particular, some MOFs materials are excited under light irradiation and exhibit photocatalytic properties similar to semiconductors. In addition, MOFs with high specific surface area can be used as ideal photocatalyst carriers to avoid the problem of nanoscale catalyst particle cluster aggregation, or combined with other photocatalysts to improve their photocatalytic activity and stability. Among them, the Zr-based MOFs material UiO-66 has attracted widespread attention due to its high specific surface area, good chemical durability and ability to absorb visible light.

[0003] However, the inefficient transfer of electrons between the MOFs structural framework and homogeneous components and the slow mass transfer process within the MOFs pores severely restrict the photocatalytic activity of MOFs. Therefore, how to functionalize a single MOFs structure becomes the key to solving the problem. Summary of the invention

[0004] The purpose of the present invention is to provide a method for producing a 4+ Partial replacement of Zr in UiO-66 4+ The invention discloses a preparation method of a UiO-66 (Zr / Hf)-based adsorption material and an application of the adsorption material, so that the adsorption material can be used for photocatalytic degradation of organic pollutants (such as phenol, etc.) in water, and can effectively improve the adsorption capacity and catalytic activity of the photocatalytic degradation material.

[0005] The technical solution of the present invention: A method for preparing a UiO-66-based adsorption material for photocatalysis comprises the following steps: S1, adding an organic ligand and zirconium chloride into a DMF solvent, adding acetic acid, and after a hydrothermal reaction, drying the solid product to obtain a UiO-66-based material; S2, hafnium chloride is dispersed in anhydrous dichloroethane, and then THF and n-hexane dried over Na are added, and the mixture is reacted at 0°C under N2 protection to obtain a yellow precipitate HfCl4(THF)2, which is then filtered, washed and dried; S3, UiO-66-based material, HfCl4(THF)2 and DMF were mixed, reacted at 120 °C for 5-20 h, and the solid product was washed and vacuum dried to obtain Hf 4+ Partial replacement of Zr in UiO-66 4+ UiO-66 (Zr / Hf) based materials; Wherein, the organic ligand in step S1 includes one or more of terephthalic acid, 2-aminoterephthalic acid, and 2,5-dihydroxyterephthalic acid, and the molar ratio of zirconium chloride to the organic ligand is 1-5:1; the amount of DMF and acetic acid added is: 20-60 mL DMF and 1-3 mL acetic acid are added per mol of zirconium chloride.

[0006] Wherein, the hydrothermal reaction conditions in step S1 are 120° C. and 72 h.

[0007] The solid product in step S1 was washed three times with DMF and methanol respectively, and the drying condition was 60° C. for 24 h.

[0008] Wherein, the volume ratio of anhydrous dichloroethane, THF and n-hexane in step S2 is 50:8.6:100, and the amount of hafnium chloride added is: 0.1-1 g of hafnium chloride is added per 100 ml of n-hexane; the yellow precipitate HfCl4(THF) obtained by the reaction is 2, The samples were washed twice with n-hexane and dried at 60 °C for 3 h.

[0009] Among them, the mass ratio of UiO-66-based material and HfCl4(THF)2 in step S3 is 1:1~2, and the amount of DMF added in the reaction is: 15~20 mL of DMF is added for every 1g of UiO-66-based material; the solid product is washed 3 times with DMF and ethanol respectively, and the vacuum drying conditions are 40°C for 24 h.

[0010] The technical solution of the present invention also includes: a UiO-66 (Zr / Hf) based adsorption material for photocatalysis prepared by the above method.

[0011] The technical solution of the present invention also includes: application of the above-mentioned UiO-66 (Zr / Hf) based adsorption material for photocatalysis in photocatalytic degradation of organic pollutants in water.

[0012] The beneficial effects of the present invention are: The present invention adopts Hf 4+ Partial replacement of Zr in UiO-66 4+ , forming Hf 4+ -O-Zr 4+ structure, reducing the bandgap bandwidth, adding Hf 4+ Acts as a medium to promote the transfer of electrons from the ligand to Zr 4+ The active site moves, and this oxygen bridge structure can effectively enhance the photocatalytic degradation performance of the catalyst. Due to the thermal and chemical stability of the metal organic framework material UiO-66, it can stably exist in media such as acid and water, which can effectively broaden its application scenarios. In addition, the organic matter degradation rate of the catalyst using the material of the present invention can be increased by 4~11% compared with other catalysts such as Cu / g-C3N4~75%. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a transmission electron micrograph of the UiO-66 (Zr / Hf) photocatalyst prepared in Example 1.

[0014] Figure 2 This is a transmission electron micrograph of the UiO-66 (Zr / Hf) photocatalyst prepared in Example 2.

[0015] Figure 3 This is a transmission electron microscopy image of the UiO-66 (Zr / Hf) photocatalyst prepared in Example 3.

[0016] Figure 4 This is a transmission electron microscopy image of the UiO-66 photocatalyst prepared in comparative example.

[0017] Figure 5 This is a diagram showing the degradation effect of the UiO-66 (Zr / Hf) photocatalyst prepared in Examples 1 to 3 on phenol. DETAILED DESCRIPTION

[0018] The technical solution of the present invention is further described below in conjunction with specific embodiments. Example

[0019] The present invention provides a method for preparing a UiO-66-based adsorption material for photocatalytic degradation of organic pollutants in water, specifically comprising: 2 mol of zirconium chloride and 1 mol of terephthalic acid were added to 60 mL of DMF and stirred at room temperature for 30 min. After the zirconium chloride was fully dissolved, 3.5 mL of acetic acid was added and stirred for another 30 min. The above solution was transferred to a polytetrafluoroethylene liner and reacted at 120 °C for 72 h under hydrothermal conditions. After the reaction, a brown precipitate was filtered to obtain the precipitate, which was washed with DMF and methanol for 3 times, centrifuged, and dried at 60 °C for 24 h to obtain sample A (UiO-66); 0.3 g of hafnium chloride was added to 50 mL of anhydrous dichloroethane, and then 8.6 mL of THF and 100 mL of anhydrous n-hexane (Na drying) were added, and the reaction was carried out at 0 °C for 3 h under N2 protection, and then a yellow precipitate was obtained after filtering, which was washed with n-hexane twice and dried at 60 °C for 3 h to obtain sample B (HfCl4(THF)2); 0.28 g of sample A and 0.28 g of sample B were added to 7 mL of DMF, reacted at 120 °C for 5 h, centrifuged after the reaction, washed with DMF and ethanol for 3 times, and dried at 40 °C for 24 h to obtain the adsorption material of the present invention, such as Figure 1 .

[0020] This example also investigates the ability of the prepared UiO-66 (Zr / Hf) based adsorption material to photocatalytically degrade p-phenol under visible light, and the specific steps are as follows: 50 mg of UiO-66 (Zr / Hf) based adsorption material was added as a photocatalyst to 100 mL of 10 mg / L phenol ethanol solution. The solution was balanced in a dark environment for 30 min. A 300 W xenon lamp was used as the light source. The photocatalytic degradation reaction was carried out at room temperature. Samples were taken every 30 min and the concentration of the samples was measured using an ultraviolet spectrophotometer. The results are shown in Figure 2. Figure 5 shown.

[0021] from Figure 5 It can be seen that the degradation rate of p-phenol by the UiO-66 (Zr / Hf) photocatalyst prepared in this example is 86.1% within 4 h. Example

[0022] The present invention provides a method for preparing a UiO-66-based adsorption material for photocatalytic degradation of organic pollutants in water, specifically comprising: 3 mol of zirconium chloride, 1 mol of zirconium chloride terephthalate and 2-aminoterephthalic acid were added to 70 mL of DMF and stirred at room temperature for 30 min. After the zirconium chloride was fully dissolved, 3.5 mL of acetic acid was added and stirred for another 30 min. The above solution was transferred to a polytetrafluoroethylene liner and reacted at 120 °C for 72 h under hydrothermal conditions. After the reaction, a brown precipitate was filtered to obtain the brown precipitate, which was washed with DMF and methanol for 3 times, centrifuged, and dried at 60 °C for 24 h to obtain sample A (UiO-66-NH2); 0.4 g of hafnium chloride was added to 50 mL of anhydrous dichloroethane, and then 8.6 mL of THF and 100 mL of anhydrous n-hexane (Na drying) were added, and the mixture was reacted at 0 °C for 3 h under N2 protection, and then filtered to obtain a yellow precipitate, which was washed with n-hexane twice and dried at 60 °C for 3 h to obtain sample B (HfCl4(THF)2); 0.28 g of sample A and 0.34 g of sample B were added to 7 mL of DMF, reacted at 120 °C for 10 h, centrifuged after the reaction, washed with DMF and ethanol for 3 times, and dried at 40 °C for 24 h to obtain the UiO-66-NH2 (Zr / Hf) adsorption material of the present invention, such as Figure 2 .

[0023] This example also investigates the ability of the prepared UiO-66 (Zr / Hf) based adsorption material to photocatalytically degrade p-phenol under visible light, and the specific steps are as follows: 50 mg of UiO-66 (Zr / Hf) based adsorption material was added as a photocatalyst to 100 mL of 10 mg / L phenol ethanol solution. The solution was balanced in a dark environment for 30 min. A 300 W xenon lamp was used as the light source. The photocatalytic degradation reaction was carried out at room temperature. Samples were taken every 30 min and the concentration of the samples was measured using an ultraviolet spectrophotometer. The results are shown in Figure 2. Figure 5 shown.

[0024] from Figure 5 It can be seen that the degradation rate of p-phenol by the UiO-66 (Zr / Hf) photocatalyst prepared in this example is 81.3% within 4 h. Example

[0025] The present invention provides a method for preparing a UiO-66-based adsorption material for photocatalytic degradation of organic pollutants in water, specifically comprising: 4 mol of zirconium chloride, 1 mol of zirconium chloride terephthalate and 2,5-dihydroxyterephthalic acid were added to 80 mL of DMF and stirred at room temperature for 30 min. After the zirconium chloride was fully dissolved, 3.5 mL of acetic acid was added and stirred for another 30 min. The above solution was transferred to a polytetrafluoroethylene liner and reacted at 120 °C for 72 h under hydrothermal conditions. After the reaction, a brown precipitate was filtered to obtain the brown precipitate, which was washed with DMF and methanol three times, centrifuged, and dried at 60 ° C for 24 h to obtain sample A (UiO-66-(OH)2); 0.5 g of hafnium chloride was added to 50 mL of anhydrous dichloroethane, and then 8.6 mL of THF and 100 mL of anhydrous n-hexane (Na drying) were added, and the mixture was reacted at 0 ° C for 3 h under N2 protection, and then filtered to obtain a yellow precipitate, which was washed with n-hexane twice and dried at 60 ° C for 3 h to obtain sample B (HfCl4(THF)2); 0.28 g of sample A and 0.56 g of sample B were added to 7 mL of DMF, reacted at 120 ° C for 15 h, centrifuged after the reaction, washed with DMF and ethanol three times, and dried at 40 ° C for 24 h to obtain the UiO-66-(OH)2 (Zr / Hf) adsorption material of the present invention, such as Figure 3 .

[0026] This example also investigates the ability of the prepared UiO-66 (Zr / Hf) based adsorption material to photocatalytically degrade p-phenol under visible light, and the specific steps are as follows: 50 mg of UiO-66 (Zr / Hf) based adsorption material was added as a photocatalyst to 100 mL of 10 mg / L phenol ethanol solution. The solution was balanced in a dark environment for 30 min. A 300 W xenon lamp was used as the light source. The photocatalytic degradation reaction was carried out at room temperature. Samples were taken every 30 min and the concentration of the samples was measured using an ultraviolet spectrophotometer. The results are shown in Figure 2. Figure 5 shown.

[0027] from Figure 5 It can be seen that the degradation rate of p-phenol by the UiO-66 (Zr / Hf) photocatalyst prepared in this example is 79.2% within 4 h.

Claims

1. A method for preparing a UiO-66-based adsorption material for photocatalysis, characterized in that: Includes the following step, S1, adding an organic ligand and zirconium chloride into a DMF solvent, adding acetic acid, and after a hydrothermal reaction, drying the solid product to obtain a UiO-66-based material; S2, hafnium chloride is dispersed in anhydrous dichloroethane, and then THF and n-hexane dried over Na are added, and the mixture is reacted at 0°C under N2 protection to obtain a yellow precipitate HfCl4(THF)2, which is then filtered, washed and dried; S3, UiO-66-based material, HfCl4(THF)2 and DMF were mixed, reacted at 120 °C for 5-20 h, and the solid product was washed and vacuum dried to obtain Hf 4+ Partial replacement of Zr in UiO-66 4+ UiO-66 (Zr / Hf) based materials.

2. The method for preparing the UiO-66-based adsorption material for photocatalysis according to claim 1, characterized in that: The organic ligand in step S1 includes one or more of terephthalic acid, 2-aminoterephthalic acid, and 2,5-dihydroxyterephthalic acid, and the molar ratio of zirconium chloride to the organic ligand is 1-5:1; the amount of DMF and acetic acid added is: 20-60 mL DMF and 1-3 mL acetic acid per mol of zirconium chloride.

3. The method for preparing the UiO-66-based adsorption material for photocatalysis according to claim 1, characterized in that: The hydrothermal reaction conditions in step S1 are 120° C. and 72 h.

4. The method for preparing the UiO-66-based adsorption material for photocatalysis according to claim 1, characterized in that: The solid product in step S1 was washed three times with DMF and methanol respectively, and dried at 60°C for 24 h.

5. The method for preparing the UiO-66-based adsorption material for photocatalysis according to claim 1, characterized in that: The volume ratio of anhydrous dichloroethane, THF and n-hexane in step S2 is 50:8.6:100, and the amount of hafnium chloride added is: 0.1-1 g of hafnium chloride is added per 100 ml of n-hexane; the yellow precipitate HfCl4(THF) obtained by the reaction is 2, The samples were washed twice with n-hexane and dried at 60 °C for 3 h.

6. The method for preparing the UiO-66-based adsorption material for photocatalysis according to claim 1, characterized in that: Step S3 The mass ratio of UiO-66-based material and HfCl4(THF)2 is 1:1~2, and the amount of DMF added in the reaction is: 15~20 mL of DMF per 1 g of UiO-66-based material; the solid product is washed three times with DMF and ethanol respectively, and the vacuum drying conditions are 40 ℃ for 24 h.

7. A UiO-66 (Zr / Hf) based adsorption material for photocatalysis prepared by the method of any one of claims 1 to 6.

8. Use of the UiO-66 (Zr / Hf) based adsorption material for photocatalysis according to claim 7 in photocatalytic degradation of organic pollutants in water.

Citation Information

Patent Citations

  • Synthesis of improved metallocene catalyst as well as synthesis equipment and application of improved metallocene catalyst

    CN114195920A

  • UiO-66 material, preparation method and application of UiO-66 material in removal of organic pollutants through synergism of thermotropic adsorption and photocatalysis

    CN117186428A

  • METHOD FOR PRODUCTION OF HAFNIUM COMPOUND, HAFNIUM COMPOUND WITH IMPURITY Zr OF 50 PPM OR LESS, AND METHOD OF FORMING HAFNIUM-BASED FILM

    JP2007051042A