Preparation method of high-low temperature alternating low-friction solid lubricating coating
The preparation of high-temperature solid lubricating coatings by hydrothermal synthesis of silicate nanomaterials has been solved, and the problem of insufficient friction performance under high temperature conditions in the prior art has been achieved, low friction lubrication effect in a wide temperature range is achieved, and the use of equipment has been extended. life.
Patent Information
- Application Number
- CN202410900256.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing high-temperature solid lubricating coatings have insufficient friction performance under high temperature conditions and lack temperature adaptability, so they cannot maintain low friction lubricating performance at different temperatures.
The silicate nanomaterials are synthesized as lubricating phases, and the silicate nanopowder is prepared by ball milling and magnetic stirring, and mixed with binder and organic solvents. It is prepared on the metal surface by atmospheric spraying or brushing. Solid lubricating coating with temperature adaptability and low friction properties.
Low friction performance is achieved in the range of 20 to 600°C, reducing the friction coefficient to less than 0.01, significantly reducing wear and extending the service life of the equipment.
Smart Images

Figure CN118976683A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a high-low temperature alternating low-friction solid lubricating coating, belonging to the technical field of high-temperature solid lubricating coatings. Background Art
[0002] Solid lubricating coating is one of the key technologies for reliable operation of motion mechanisms in aerospace engineering and military equipment. It is mainly used in high / low temperature, vacuum, strong radiation and other occasions, as well as in mechanical equipment such as corrosive media, electrical contacts, and thermal processing of certain metals or plastic materials. With the development of my country's new generation of aerospace equipment and armed combat equipment, solid lubricating coatings will withstand higher and wider operating temperatures, greater impact loads and frequencies, liquid media, and multiple service environments such as atmosphere-vacuum radiation and other harsh working conditions.
[0003] Whether the lubricating phase material in the solid lubricating coating can withstand high temperature, or whether it can adaptively generate substances with lubricating function at different temperatures is the decisive factor for the high-temperature tribological performance of the coating. Currently, these lubricating phase materials mainly include transition metal sulfides (MoS2 and WS2, etc.), graphite, DLC materials, low melting point metals and friction self-generated composite oxides.
[0004] CN111853516A discloses a method for obtaining a two-dimensional composite super-lubricating surface on an engineering substrate, the method comprising a step of preparing a two-dimensional lubricant compound dispersion, wherein the two-dimensional lubricant compound material comprises any one of MoS2, WS2, TaS2, WSe2, TaSe2, NbS2, NbSe2, α-ZrP, graphene, h-BN, mica, and black phosphorus. According to the working conditions for achieving super-lubrication of the two-dimensional composite super-lubricating surface, the influence of temperature is not emphasized; according to the type of two-dimensional nanomaterials selected, it is inferred that it does not have high-temperature super-lubricating properties (for example, transition element sulfides are prone to high-temperature oxidation failure in the atmospheric environment, and carbon-based materials are not easy to shear in a vacuum environment, etc.). CN110382633A discloses a lubricating coating containing graphene, and the solid lubricant disclosed in the method is selected from wax, modified wax, PE, PP, PA, silicone wax, PTFE, polyfluorinated compounds, graphite, molybdenum disulfide, hexagonal boron nitride, tin sulfide, zinc sulfide, tungsten disulfide, metal sulfide, calcium phosphate, silicate, phyllosilicate, talc or mica. It can be seen that the coating disclosed in the method is a multiphase lubricating coating, and silicate, phyllosilicate, talc or mica are all natural mineral materials, which is obviously different from the artificial hydrothermal synthesis of silicate nanomaterials involved in the patent of this application; at the same time, the method does not mention the temperature adaptability of the coating and whether the friction performance under different temperature conditions can achieve low friction lubrication. The above solid lubricating coating-related patents are obviously different from the solid coating lubricating phase material in the present application, which is a silicate nanomaterial, and does not need to be compounded with other two-dimensional nanomaterials, and is specifically realized as low friction lubrication under high temperature conditions. Summary of the invention
[0005] In order to overcome the shortcomings of the existing high-temperature solid lubricating coating technology, the purpose of the present invention is to develop a solid lubricating coating using hydrothermally synthesized silicate nanomaterials as a high-temperature lubricating phase, in the hope of obtaining a high-temperature lubricating coating with better tribological properties.
[0006] A method for preparing a high-low temperature alternating low-friction solid lubricating coating comprises the following steps:
[0007] Step (1), weighing a certain mass ratio of carbon material, magnesium-containing compound, and silicon-containing compound, mixing and ball-milling different powders, and then adding them to an alkaline solution of a predetermined concentration in a certain mass ratio; placing the obtained mixed solution in a closed reactor, setting the reaction time, reaction temperature, and reaction pressure, and magnetically stirring the entire reaction system at the same time, setting the stirring speed; naturally cooling to room temperature after the reaction is completed, and drying the mixed solution after the reaction at a set temperature to obtain silicate nanopowder or carbon-doped silicate nanopowder;
[0008] Step (2), setting the mass ratio of the binder and the organic solvent, mixing the two, and setting the stirring speed, stirring time and stirring temperature for magnetic stirring to obtain the solvent system required for coating preparation; setting the mass ratio of the silicate material and the solvent, weighing a certain mass of a silicate nanomaterial obtained in step (1) into the obtained solvent system, and setting the high-energy ball milling time to disperse the solid lubricating coating slurry;
[0009] Step (3), using atmospheric spraying or brushing and setting preparation parameters, performing step (2) to obtain the coating slurry on the metal surface pretreated by sandblasting and cleaning to initially obtain a composite solid lubricating coating; moving the metal material coated with the composite solid lubricating coating into a drying oven, drying it at a predetermined temperature, and obtaining a solid lubricating coating with temperature-adaptive super-lubricity.
[0010] In the step (1), the carbon material includes bulk graphite, graphene, graphene oxide, and microcrystalline graphite; the magnesium-containing compound includes magnesium oxide, magnesium hydroxide, magnesium silicate, and magnesium chloride; and the silicon-containing compound includes silicon dioxide and sodium silicate.
[0011] In the step (1), the reaction time is 6 to 60 hours, the reaction temperature is 160 to 320° C., and the reaction pressure is 1.6 to 3.8 MPa.
[0012] In the step (1), the mass ratio of the magnesium-containing compound, the silicon-containing compound, and the carbon material is 1:1:0.01-0.1; and the pH value of the alkaline solution is 13-14.
[0013] In the step (1), the reaction time is 6 to 60 hours, the reaction temperature is 160 to 320° C., and the reaction pressure is 1.6 to 3.8 MPa.
[0014] In the step (2), the binder includes: epoxy resin, phenolic resin, polyimide, aluminum dihydrogen phosphate; the organic solvent includes: water, alcohol, acetone, petroleum ether, dimethylformamide.
[0015] In the step (2), the mass ratio of the binder to the organic solvent is 1:5-20; and the stirring temperature is 20-100°C.
[0016] In the step (2), the mass ratio of the silicate nanomaterial to the solvent system is 1:3-10; and the high-energy ball milling time is 30 minutes with a 3-minute interval between each 10-minute ball milling.
[0017] In the step (3), the spraying pressure of the atmospheric spraying method is 0.6-2 MPa; the coating thickness of the brush coating method is 10-100 μm.
[0018] In the step (3), the coating drying process is 80, 100, 120, 140, 160, 180°C for 0-2h each and 200°C for 0-2h.
[0019] The advantage of the present invention is that the method for preparing an alternating high and low temperature low friction silicate solid lubricating coating on the surface of a metal substrate that can achieve a temperature range of 20 to 600°C is simple and reliable. The prepared solid lubricating coating exhibits particularly excellent tribological properties under atmospheric high temperature / low temperature reciprocating cycle conditions, can reduce the friction coefficient to below 0.01, significantly reduce wear, make the machine run smoothly, and greatly extend the service life of the equipment.
[0020] The invention has strong operability, and the thickness of the obtained solid lubricating coating can be controlled by controlling the coating formula and coating preparation parameters. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] When considered in conjunction with the accompanying drawings, the present invention can be more completely and better understood and many of the accompanying advantages can be easily known by referring to the detailed description below, but the drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention, as shown in the figure:
[0022] Figure 1 This is a scanning electron microscope image of a hydrothermally synthesized silicate nanomaterial used in the preparation of a high-low temperature alternating low-friction solid lubricating coating in Example 1 of the present invention;
[0023] Figure 2 This is a surface scanning electron microscope image of a high-low temperature alternating low-friction solid lubricating coating according to Example 1 of the present invention;
[0024] Figure 3 This is a cross-sectional scanning electron microscope image of a high-low temperature alternating low-friction solid lubricating coating according to Example 1 of the present invention.
[0025] Figure 4 This is a friction coefficient curve of a high-low temperature alternating low-friction solid lubricating coating in Example 1 of the present invention in an atmospheric high-temperature-low-temperature reciprocating environment.
[0026] Figure 5 This is a scanning electron microscope image of a hydrothermally synthesized carbon-doped silicate nanomaterial used in the preparation of a high-low temperature alternating low-friction solid lubricating coating in Example 2 of the present invention;
[0027] Figure 6 This is a transmission electron microscope image of a hydrothermally synthesized carbon-doped silicate nanomaterial used in the preparation of a high-low temperature alternating low-friction solid lubricating coating in Example 2 of the present invention;
[0028] Figure 7 This is a cross-sectional scanning electron microscope image of a high-low temperature alternating low-friction solid lubricating coating according to Example 2 of the present invention;
[0029] Figure 8 This is a surface scanning electron microscope image of a high-low temperature alternating low-friction solid lubricating coating according to Example 2 of the present invention.
[0030] Fig. 9 This is a friction coefficient curve of a high-low temperature alternating low-friction solid lubricating coating in Example 2 of the present invention after undergoing reciprocating friction in an atmospheric low-temperature-high-temperature-low-temperature thermal cycle (20-600-20°C) in the atmosphere at 600°C.
[0031] The present invention is further described below in conjunction with the accompanying drawings and embodiments. DETAILED DESCRIPTION
[0032] Obviously, many modifications and changes made by those skilled in the art based on the purpose of the present invention belong to the protection scope of the present invention.
[0033] It will be understood by those skilled in the art that, unless expressly stated, the singular forms "a", "an", "said" and "the" used herein may also include plural forms. It should be further understood that the term "comprising" used in this specification refers to the presence of the features, integers, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof. It should be understood that when an element or component is said to be "connected" to another element or component, it may be directly connected to the other element or component, or there may be an intermediate element or component. The term "and / or" used herein includes any unit and all combinations of one or more associated listed items.
[0034] It should be understood by those skilled in the art that unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those skilled in the art to which this invention belongs.
[0035] To facilitate understanding of the embodiments of the present invention, further explanations will be given below, and each embodiment does not constitute a limitation on the embodiments of the present invention.
[0036] Embodiment 1: A high-low temperature alternating super-slip solid lubricating coating, comprising the following steps:
[0037] The selected metal material is copper material, the selected binder is phenolic resin, the selected organic solvent is dimethylformamide, and the solid lubricating material is flaky hydroxy magnesium silicate nano material.
[0038] The mass ratio of phenolic resin: dimethylformamide: hydroxy magnesium silicate is 5:25:3, and the selected spraying method is atmospheric spraying.
[0039] Specifically, magnesium oxide and silicon dioxide were selected as raw materials for the hydrothermal reaction, sodium hydroxide was used as the reaction medium, the mass ratio of magnesium oxide to silicon dioxide was set to 1:1, the pH value of the hydrothermal solution was 14, the hydrothermal temperature was 200°C, the hydrothermal pressure was 1.6 MPa, the hydrothermal time was 12 h, and the drying temperature was 80°C to prepare flaky magnesium hydroxysilicate nanomaterials; copper metal materials were selected, and their surfaces were sandblasted using sandpaper and a polishing machine until the roughness reached Ra 0.3, then use alcohol or acetone to ultrasonically clean the metal material to remove oil or impurities on its surface; weigh 1g of thermoplastic phenolic resin powder and 5g of dimethylformamide solvent respectively, set the stirring speed to 200rpm and the stirring time to 30min to fully mix the two with magnetic stirring; weigh 1.67g of flaky hydroxy magnesium silicate powder in an organic solvent, set the stirring speed to 200rpm and the stirring time to 30min to fully disperse the powder in the liquid; set the spray gun pressure to 0.8MPa, the vertical spray distance to 30cm, and the spray gun moving speed to 30cm / s, and spray the coating material on the surface of the metal substrate; after spraying, set the drying box temperature to 180℃ and the drying time to 2h to obtain a composite solid lubricating coating that can achieve temperature-adaptive super-lubricity.
[0040] The solid lubricating phase in the environmentally adaptive super-slip solid lubricating coating is a sheet-like hydroxy magnesium silicate nanomaterial prepared by a hydrothermal method. The electron microscopic morphology is shown in FIG. Figure 1 The surface microstructure and cross-sectional microstructure of the coating are shown in Figure 2 and Figure 3 shown.
[0041] from Figure 1 It can be seen that the hydroxy magnesium silicate nanopowder obtained by the present invention has a microscopic flake morphology, an average lateral radius of 30 to 50 nm, and a thickness of about 10 nm. Figure 2 and Figure 3 It can be seen that the solid lubricating coating obtained by the implementation of the present invention contains fewer holes and crack defects and has a thickness of about 60 μm.
[0042] from Figure 4 It can be seen that the solid lubricating coating obtained by the implementation of the present invention can make the friction coefficient of the friction pair no longer affected by temperature after multiple temperature change cycles of 20 to 400° C., and can achieve ultra-low friction (<0.01) in a wider temperature range.
[0043] Embodiment 2: A high-low temperature alternating low-friction solid lubricating coating, comprising the following steps:
[0044] The selected metal material is titanium alloy material, the selected binder is aluminum dihydrogen phosphate, the selected organic solvent is water, and the solid lubricating material is carbon-doped hydroxy magnesium silicate nanomaterial.
[0045] The mass ratio of aluminum dihydrogen phosphate: water: carbon-doped hydroxy magnesium silicate is 6:35:7, and a brush coating method is selected to prepare the coating.
[0046] Specifically, magnesium oxide, silicon dioxide, and bulk graphite were selected as raw materials for hydrothermal reaction, sodium hydroxide was used as reaction medium, and the mass ratio of magnesium oxide, silicon dioxide, and bulk graphite was set to 1:1:0.1, the pH value of the hydrothermal solution was 14, the hydrothermal temperature was 300°C, the hydrothermal pressure was 3.6MPa, the hydrothermal time was 48h, and the drying temperature was 80°C to prepare carbon-doped hydroxy magnesium silicate nanomaterials; titanium alloy metal blocks were selected, and their surfaces were sandblasted using sandpaper and a polishing machine until the roughness reached Ra 0.1, then use alcohol or acetone to ultrasonically clean the metal material to remove oil or impurities on its surface; weigh 12g of aluminum dihydrogen phosphate and 70g of distilled water respectively, set the stirring speed to 200rpm, the stirring time to 60min, and the temperature to 100℃ to fully mix the two with magnetic stirring; weigh 14g of carbon-doped hydroxy magnesium silicate powder in the solvent, set the stirring speed to 200rpm, and the stirring time to 30min to fully disperse the powder in the liquid; set the brushing thickness to 60μm, and brush the coating material on the surface of the metal substrate; after completion, set the drying box temperature to 80, 100, 120, 140, 160, and 180℃ for drying for 1h each, and 200℃ for drying for 2h to obtain a composite solid lubricating coating that can achieve temperature-adaptive low friction of 20~600℃.
[0047] The solid lubricating phase in the environmentally adaptive low-friction solid lubricating coating is a tan-doped hydroxy magnesium silicate nanomaterial prepared by a hydrothermal method. The electron microscopic morphology is shown in FIG. Figure 5 and Figure 6 The surface microstructure and cross-sectional microstructure of the coating are shown in Figure 7 and Figure 8 shown.
[0048] from Figure 5 and Figure 6 It can be seen that the carbon-doped magnesium silicate hydroxy nanopowder obtained by the present invention has a microscopic flake morphology, an average lateral radius of about 300nm, a thickness of 10-22nm, and is coated with a graphene-like carbon layer structure with a nanometer-level thickness. Figure 7 and Figure 8 It can be seen that the solid lubricating coating obtained by the implementation of the present invention contains a certain amount of defects such as holes, bubbles and cracks, presents a loose structure, and has a thickness of about 60 μm.
[0049] from Fig. 9It can be seen that the solid lubricating coating obtained by the implementation of the present invention has a friction coefficient of the friction pair maintained at about 0.25 after a temperature change cycle of 20-600°C.
Claims
1. A method for preparing a high-low temperature alternating low-friction solid lubricating coating, characterized in that The following steps are involved: Step (1), preparation of silicate nanopowder and carbon-doped silicate nanopowder with a particle size of less than 50 nm in a certain direction: weigh a certain mass of carbon material, magnesium-containing compound, and silicon-containing compound, mix the three powders and ball-mill them, and then add them to an alkaline solution of a predetermined concentration in a certain mass ratio; place the obtained mixed solution in a closed reactor, set the reaction time, reaction temperature, and reaction pressure, and simultaneously perform magnetic stirring on the entire reaction system and set the stirring speed; after the reaction is completed, naturally cool to room temperature, set the temperature to dry the mixed solution after the reaction, and obtain nanopowder; Step (2), configuration of the high-low temperature alternating low-friction solid lubricating coating slurry: setting the mass ratio of the binder and the organic solvent, mixing the two, and setting the stirring speed, stirring time and stirring temperature to perform magnetic stirring to obtain the solvent system required for coating preparation; setting the mass ratio of the silicate material and the solvent, weighing a certain mass of a certain silicate nanomaterial obtained in step (1) into the obtained solvent system, setting the high-energy ball milling time to perform magnetic stirring on the solid lubricating coating slurry; Step (3), preparation of a high-low temperature alternating low-friction solid lubricating coating: using an atmospheric spraying method or a brush coating method and setting preparation parameters, the coating slurry obtained in step (2) is prepared on a metal surface pretreated by sandblasting and cleaning to preliminarily obtain a composite solid lubricating coating; The metal material coated with the composite solid lubricating coating is moved into a drying box and dried at a predetermined temperature to obtain a temperature-adaptive super-lubricating solid lubricating coating.
2. The method for preparing a high-low temperature alternating low-friction solid lubricating coating according to claim 1, characterized in that In the step (1), the carbon material includes bulk graphite, graphene, graphene oxide, and microcrystalline graphite.
3. The method for preparing a high-low temperature alternating low-friction solid lubricating coating according to claim 1, characterized in that In the step (1), the magnesium-containing compound includes: magnesium oxide, magnesium hydroxide, magnesium silicate, magnesium chloride; the silicon-containing compound includes silicon dioxide, sodium silicate.
4. The method for preparing a high-low temperature alternating low-friction solid lubricating coating according to claim 1, characterized in that In the step (1), the mass ratio of the magnesium-containing compound, the silicon-containing compound, and the carbon material is 1:1:0.01-0.1; and the pH value of the alkaline solution is 13-14.
5. The method for preparing a high-low temperature alternating low-friction solid lubricating coating according to claim 1, characterized in that In the step (1), the reaction time is 6 to 60 hours, the reaction temperature is 160 to 320° C., and the reaction pressure is 1.6 to 3.8 MPa.
6. The method for preparing a high-low temperature alternating low-friction solid lubricating coating according to claim 1, characterized in that In the step (2), the binder includes: epoxy resin, phenolic resin, polyimide, aluminum dihydrogen phosphate; the organic solvent includes: water, alcohol, acetone, petroleum ether, dimethylformamide.
7. The method for preparing a high-low temperature alternating low-friction solid lubricating coating according to claim 1, characterized in that In the step (2), the mass ratio of the binder to the organic solvent is 1:5-20; and the stirring temperature is 20-100°C.
8. The method for preparing a high-low temperature alternating low-friction solid lubricating coating according to claim 1, characterized in that In the step (2), the mass ratio of the silicate nanomaterial to the solvent system is 1:3-10; and the high-energy ball milling time is 30 minutes with a 3-minute interval between each 10-minute ball milling.
9. The method for preparing a high-low temperature alternating low-friction solid lubricating coating according to claim 1, characterized in that In the step (3), the spraying pressure of the atmospheric spraying method is 0.6-2 MPa; the coating thickness of the brush coating method is 10-100 μm.
10. The method for preparing a high-low temperature alternating low-friction solid lubricating coating according to claim 1, characterized in that In the step (3), the coating drying process is 80, 100, 120, 140, 160, 180°C for 0.5 to 2h each and 200°C for 2h.
11. Application of the coating obtained by the method for preparing the high-low temperature alternating low-friction solid lubricating coating according to any one of claims 1 to 10 in the fields of aerospace, military equipment and transportation.
Citation Information
Patent Citations
Preparation method of hydroxyl magnesium silicate / carbon composite nano material and application thereof
CN110436444A
Preparation method of polymer-based bonded solid composite lubricating film
CN111019738A
Preparation method of temperature-adaptive super-smooth solid lubricating coating
CN115093767A
Method for preparing high-temperature super-lubricity silicate lubricating coating on surface of metal substrate
CN115233209A