Flower-shaped spherical silver powder and preparation method thereof
By preparing a solution containing silver nitrate, reducing agent and surfactant, adjusting the pH value and reacting, flower-like spherical silver powder is prepared, which solves the problem of insufficient specific surface area of silver particles and achieves silver powder with high specific surface area and good dispersion. Suitable for conductive materials and other fields.
Patent Information
- Application Number
- CN202411134220.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-19
AI Technical Summary
It is difficult to prepare silver particles with a higher specific surface area in the prior art, and the specific surface area of nanometal particles is limited due to agglomeration and bridge formation.
By preparing the first solution and the second solution, the first solution includes silver nitrate, the second solution includes a reducing agent, a dispersant and a surfactant, adjust the pH value of the second solution and add the first solution to react to obtain a silver powder suspension , and the floral spherical silver powder is separated from it, and the morphology and size of the silver powder are controlled by surfactant to avoid agglomeration and bridge effects.
The preparation of floral spherical silver powder with a large specific surface area ensures its good dispersion and uniformity, and has a wide range of application prospects in the fields of conductive pastes, conductive coatings, etc.
Smart Images

Figure CN118976906A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal powder preparation, and in particular to a flower-shaped spherical silver powder and a preparation method thereof. Background Art
[0002] In the field of metal powder preparation technology, silver powder occupies a core position in many high-tech applications such as electronic packaging, conductive coatings, and antibacterial materials due to its excellent conductivity and chemical stability. The properties and applications of silver powder depend on the size and morphology of silver particles.
[0003] However, the specific surface area of nano-metal particles is limited due to their aggregation and bridging phenomena. Therefore, how to prepare silver particles with a higher specific surface area is a problem that needs to be solved at present and in the future. Summary of the invention
[0004] The purpose of the present application is to provide a flower-shaped spherical silver powder and a preparation method thereof, so as to prepare flower-shaped spherical silver powder with a large specific surface area, thereby having good application prospects in multiple fields such as conductive pastes and conductive coatings.
[0005] The embodiment of the present application provides a method for preparing flower-shaped spherical silver powder, which comprises: preparing a first solution and a second solution, wherein the first solution comprises silver nitrate, and the second solution comprises a reducing agent, a dispersant, and a surfactant; adjusting the pH value of the second solution to a preset value, and then adding the second solution to the first solution for reaction to obtain a silver powder suspension, wherein the preset value is 3 to 7; separating flower-shaped spherical silver powder from the silver powder suspension, wherein the flower-shaped spherical silver powder is a quasi-spherical silver powder with a flower-like structure.
[0006] Among them, the mass concentration of silver nitrate in the first solution is 5-25%, the mass concentration of the reducing agent in the second solution is 10-20%; the ratio of the mass of the reducing agent in the second solution to the mass of the silver nitrate in the first solution is 50-60%; the ratio of the mass of the dispersant in the second solution to the mass of the silver nitrate in the first solution is 5-20%; the ratio of the mass of the surfactant in the second solution to the mass of the silver nitrate in the first solution is 0.5-5%.
[0007] Among them, the reducing agent includes at least one of glucose, ascorbic acid, hydrazine hydrate, hydrogen peroxide, formaldehyde and acetaldehyde; the dispersant includes at least one of polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene glycol, gum arabic, gelatin and Tween; the surfactant includes at least one of silane coupling agent, span, oleic acid, sodium dodecylbenzene sulfonate, methyl benzotriazole and benzotriazole.
[0008] Wherein, the surfactant is sodium dodecylbenzene sulfonate or benzotriazole.
[0009] Among them, after the pH value of the second solution is adjusted to a preset value, it is added to the first solution for reaction to obtain a silver powder suspension, including: after the pH value of the second solution is adjusted to a preset value by adding a pH adjuster to the second solution, it is added to the first solution for reaction to obtain a silver powder suspension; the pH adjuster includes at least one of ammonia water, sodium hydroxide, sodium bicarbonate, oxalic acid, phosphoric acid, nitric acid, hydrochloric acid and sulfuric acid.
[0010] Among them, after the pH value of the second solution is adjusted to a preset value, it is added to the first solution for reaction to obtain a silver powder suspension, including: after the pH value of the second solution is adjusted to a preset value, under stirring conditions, adding it to the first solution for reaction within a preset addition time to obtain a silver powder suspension, and the preset addition time is 5 to 15 minutes.
[0011] Among them, after the pH value of the second solution is adjusted to a preset value, it is added to the first solution for reaction to obtain a silver powder suspension, including: after the pH value of the second solution is adjusted to a preset value, it is added to the first solution for reaction under preset reaction temperature conditions to obtain a silver powder suspension, and the preset reaction temperature is 25-45°C.
[0012] The method comprises separating flower-shaped spherical silver powder from a silver powder suspension, comprising: separating the silver powder suspension into solid and liquid, washing the separated solid, and drying the washed solid at a drying temperature of 40 to 60° C. for a drying time of 60 to 120 minutes to obtain flower-shaped spherical silver powder.
[0013] Among them, the specific surface area of the flower-shaped spherical silver powder is greater than or equal to 0.9m 2 / g.
[0014] The embodiment of the present application also provides a flower-shaped spherical silver powder, which is prepared by any of the above-mentioned methods for preparing the flower-shaped spherical silver powder.
[0015] The flower-shaped spherical silver powder and the preparation method thereof provided by the present application are prepared by preparing a first solution and a second solution, wherein the first solution includes silver nitrate, and the second solution includes a reducing agent, a dispersant and a surfactant, and then the pH value of the second solution is adjusted to a preset value and then added to the first solution for reaction to obtain a silver powder suspension, wherein the preset value is 3 to 7, and then the flower-shaped spherical silver powder is separated from the silver powder suspension, wherein the flower-shaped spherical silver powder is a quasi-spherical silver powder with a flower-like structure, and thus a flower-shaped spherical silver powder with a large specific surface area can be prepared by introducing a surfactant, and the preparation process is simple, and the morphology and size of the flower-shaped spherical silver powder can be effectively regulated by changing the amount and / or type of the surfactant, and the flower-shaped spherical silver powder can effectively avoid agglomeration and bridging effects, thereby ensuring good dispersibility and uniformity of the flower-shaped spherical silver powder, and has good application prospects in multiple fields such as conductive pastes and conductive coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The technical solution and other beneficial effects of the present application will be made apparent by describing in detail the specific implementation methods of the present application in conjunction with the accompanying drawings.
[0017] Figure 1 It is a schematic flow chart of a method for preparing flower-shaped spherical silver powder provided in an embodiment of the present application;
[0018] Figure 2 is a scanning electron microscope image of the flower-shaped spherical silver powder prepared by the method for preparing the flower-shaped spherical silver powder provided in Example 1 of the present application;
[0019] Figure 3 is a scanning electron microscope image of the flower-shaped spherical silver powder prepared by the method for preparing the flower-shaped spherical silver powder provided in Example 2 of the present application;
[0020] Figure 4 This is a scanning electron microscope image of the flower-shaped spherical silver powder prepared by the method for preparing the flower-shaped spherical silver powder provided in Example 3 of the present application. DETAILED DESCRIPTION
[0021] The present application is further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present application, but are not intended to limit the scope of the present application. Similarly, the following examples are only some embodiments of the present application rather than all embodiments, and all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of this application.
[0022] In the following description of the present application, reference is made to “some embodiments”, which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.
[0023] In the following description of the present application, the terms "first\second\third" involved are merely used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged with a specific order or sequence where permitted, so that the embodiments of the present application described here can be implemented in an order other than that illustrated or described here.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.
[0025] The following is a detailed description with reference to specific embodiments. It should be noted that the serial numbers of the following embodiments are not intended to limit the preferred order of the embodiments.
[0026] See also Figure 1 , Figure 1 : is a schematic diagram of a process for preparing a flower-shaped spherical silver powder provided in an embodiment of the present application. The specific process of the method for preparing the flower-shaped spherical silver powder can be as follows:
[0027] Step S11. Prepare a first solution and a second solution, wherein the first solution includes silver nitrate, and the second solution includes a reducing agent, a dispersant, and a surfactant.
[0028] In this embodiment, the mass concentration of silver nitrate in the first solution may be 5-25%. In some examples, the mass concentration of silver nitrate in the first solution may be specifically 5-15%, for example, 5%, 10% or 15%. The mass concentration of the reducing agent in the second solution may be 10-20%, for example, 10%, 15% or 20%. The mass ratio of the reducing agent in the second solution to the mass of silver nitrate in the first solution may be 50-60%, for example, 50%, 52%, 54%, 56%, 58% or 60%. The mass ratio of the dispersant in the second solution to the mass of silver nitrate in the first solution may be 5-20%, for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%. The ratio of the mass of the surfactant in the second solution to the mass of the silver nitrate in the first solution can be 0.5-5%, for example, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5% or 5.0%, etc.
[0029] Specifically, the reducing agent may include at least one of glucose, ascorbic acid, hydrazine hydrate, hydrogen peroxide, formaldehyde and acetaldehyde, for example, ascorbic acid may be specifically used. The dispersant may include at least one of polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene glycol, gum arabic, gelatin and tween, for example, polyvinyl pyrrolidone may be specifically used. The surfactant may include at least one of silane coupling agent, span, oleic acid, sodium dodecylbenzene sulfonate, methyl benzotriazole and benzotriazole, for example, sodium dodecylbenzene sulfonate or benzotriazole may be specifically used.
[0030] In some embodiments, the method for preparing the first solution can be specifically as follows: adding silver nitrate to ultrapure water, stirring and dissolving to obtain the first solution. In a specific implementation, 5 kg of silver nitrate solid can be added to ultrapure water, stirring and dissolving to obtain a silver nitrate solution with a mass fraction of 5% (i.e., the first solution).
[0031] In some embodiments, the method for preparing the second solution can be specifically as follows: adding a reducing agent, a dispersant and an appropriate amount of a surfactant to ultrapure water, stirring and dissolving to obtain the second solution. In addition, in a specific implementation, 2.6 kg of ascorbic acid solid can be used as a reducing agent, added to ultrapure water, stirred and dissolved to obtain a reducing agent solution with a mass fraction of 15%, and then 300 g of polyvinyl pyrrolidone as a dispersant and 30 g of sodium dodecylbenzene sulfonate as a surfactant are added to the reducing agent solution, and the second solution can be obtained after stirring evenly.
[0032] In some embodiments, the method for preparing the flower-shaped spherical silver powder may further include: controlling the temperature of the first solution and the second solution at 25 to 45°C, for example, at 25°C, 30°C, 35°C, 40°C or 45°C. In this way, the reaction temperature of the first solution and the second solution in the subsequent step S12 can be controlled, and the morphology of the desired silver powder can be controlled. In addition, the inventors of the present application have found that the higher the reaction temperature of the first solution and the second solution in the subsequent step S12, the looser the aggregation of the corresponding microcrystalline silver powder.
[0033] Step S12: After adjusting the pH value of the second solution to a preset value, add the second solution to the first solution for reaction to obtain a silver powder suspension, the preset value being 3 to 7.
[0034] Among them, the preset value can be specifically 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5 or 7, etc.
[0035] In some embodiments, the above step S12 may include: adding a pH adjuster to the second solution to adjust the pH value of the second solution to a preset value, and then adding the pH adjuster to the first solution for reaction to obtain a silver powder suspension. The pH adjuster may include at least one of ammonia water, sodium hydroxide, sodium bicarbonate, oxalic acid, phosphoric acid, nitric acid, hydrochloric acid and sulfuric acid, for example, ammonia water and / or nitric acid.
[0036] In some embodiments, the above step S12 may include: adjusting the pH value of the second solution to a preset value, and then adding the second solution to the first solution for reaction under stirring conditions within a preset addition time to obtain a silver powder suspension. The preset addition time (that is, the duration of the second solution being added to the first solution) may be 5 to 15 minutes. In some examples, the preset addition time may be specifically 5 to 10 minutes, for example, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, or 10 minutes.
[0037] In some embodiments, the above step S12 may include: after adjusting the pH value of the second solution to a preset value, adding the second solution to the first solution under a preset reaction temperature to react and obtain a silver powder suspension. The preset reaction temperature may be 25 to 45°C, for example, it may be specifically 25°C, 30°C, 35°C, 40°C or 45°C, etc. Specifically, the inventors of the present application have found that the higher the preset reaction temperature (i.e., the reaction temperature of the first solution and the second solution), the looser the corresponding microcrystalline silver powder aggregation. Moreover, in a specific implementation, the reaction temperature of the first solution and the second solution prepared in the above step S11 may be controlled at the preset reaction temperature to achieve the control of the reaction temperature of the first solution and the second solution in the above step S12 at the preset reaction temperature.
[0038] In some specific embodiments, the temperature of the first solution and the second solution prepared in the above step S11 is controlled at a preset reaction temperature (for example, 25°C or 45°C), and the above step S12 may include: adding a pH adjuster (for example, ammonia water) to the second solution to adjust the pH value of the second solution to 3-7 (for example, about 5), and then adding the second solution to the first solution under stirring conditions for a feeding time of 5-10 minutes (for example, 8 minutes) to react, and continuing to stir the reaction for 5-15 minutes (for example, 10 minutes) after the addition to obtain a silver powder suspension.
[0039] Step S13: separating flower-shaped spherical silver powder from the silver powder suspension, wherein the flower-shaped spherical silver powder is a quasi-spherical silver powder with a flower-shaped structure.
[0040] It should be noted that the flower-shaped spherical silver powder obtained after the completion of the above step S13 can provide a larger specific surface area and better conductivity due to its unique structural characteristics, so it has great application potential in the fields of advanced electronic devices and high-efficiency catalysts.
[0041] Moreover, compared with the method in the related art of increasing the specific surface area of silver powder by increasing the surface roughness of silver powder, for example, by introducing a new dispersant, a crystal disruptor or other reagents to regulate the growth mode of silver powder so that it has a rough surface, the present embodiment regulates the morphology of silver powder by introducing a surfactant to control the crystal growth, which can play a similar growth regulation role on silver powder to prepare spherical silver powder with a special flower-like structure (i.e., flower-like spherical silver powder). Flower-like spherical silver powder has a rough surface and many protrusions, and thus can have a large specific surface area and high sintering activity, and has broad application prospects in the field of photovoltaic silver paste. Moreover, the raw materials used in its preparation are simple, and its preparation method is simple, which is conducive to reducing production costs.
[0042] In this embodiment, the flower-shaped spherical silver powder obtained after the above step S13 is completed has a flower-shaped structure, and its specific surface area can be greater than or equal to 0.9 m 2 / g, and it can be understood that due to the extended flower-like structure on its surface, its specific surface area is large and is beneficial to improving its sintering activity.
[0043] In some embodiments, the above step S13 may include: separating the silver powder suspension from the solid and liquid, washing the separated solid, and drying the washed solid to obtain flower-shaped spherical silver powder. The drying temperature may be 40 to 60°C, for example, 40°C, 45°C, 50°C, 55°C or 60°C. The drying time may be 60 to 120 minutes, for example, 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes, 110 minutes or 120 minutes. The method for separating the silver powder suspension from the solid and liquid may be specifically: separating the solid and liquid in the silver powder suspension by filtering. The method for washing the separated solid may be specifically: washing the separated solid with ultrapure water.
[0044] In some specific embodiments, the above step S13 may include: separating the silver powder suspension from the solid-liquid, washing the separated solid with ultrapure water, and transferring the washed solid to an oven for drying. The drying temperature may be 40 to 60° C. (for example, 60° C.), and the drying time may be 60 to 120 min (for example, 120 min). After the drying is completed, the target product (that is, the above-mentioned flower-shaped spherical silver powder) can be obtained.
[0045] It is to be understood that all raw materials used in the examples of the present application can be obtained commercially.
[0046] Furthermore, for ease of understanding, the present application is further described in detail below through three specific embodiments (ie, Embodiment 1, Embodiment 2 and Embodiment 3).
[0047] Example 1
[0048] In Example 1, the specific process of the preparation method of flower-shaped spherical silver powder can be as follows:
[0049] Step S21. preparing a first solution and a second solution, including: weighing 5 kg of silver nitrate solid to prepare a silver nitrate solution with a mass fraction of 5%, thereby obtaining a first solution; weighing 2.6 kg of ascorbic acid solid to prepare a reducing agent solution with a mass fraction of 15%, and then adding 300 g of polyvinyl pyrrolidone as a dispersant and 30 g of sodium dodecylbenzene sulfonate as a surfactant to the reducing agent solution, and stirring evenly to obtain a second solution; controlling the temperature of the first solution and the second solution at about 25°C.
[0050] Step S22. Add ammonia water to the second solution to adjust the pH value of the second solution to about 5, then add the second solution to the first solution under stirring and add the solution within 8 minutes. After adding, react for 10 minutes to obtain a silver powder suspension.
[0051] Step S23. Separate the silver powder suspension into solid and liquid, wash the separated solid with ultrapure water, and bake the washed solid in an oven at 60° C. for 120 min to obtain the target product (ie, flower-shaped spherical silver powder A1).
[0052] Specifically, the scanning electron microscope image of the flower-shaped spherical silver powder A1 (eg Figure 2 As shown in the figure, the flower-shaped spherical silver powder A1 is a quasi-spherical silver powder with a special flower-shaped structure, and its surface area is measured by gas adsorption method, and its specific surface area is 0.9 m 2 / g.
[0053] Example 2
[0054] The preparation method of the flower-shaped spherical silver powder provided in Example 2 is basically the same as the preparation method of the flower-shaped spherical silver powder provided in Example 1. The difference between the two is that the surfactant added to the reducing agent solution in Example 2 is 30 g of benzotriazole instead of 30 g of sodium dodecylbenzenesulfonate. Accordingly, in Example 2, the specific process of the preparation method of the flower-shaped spherical silver powder can be as follows:
[0055] Step S31. preparing a first solution and a second solution, including: weighing 5 kg of silver nitrate solid, preparing a silver nitrate solution with a mass fraction of 5%, so as to obtain a first solution; weighing 2.6 kg of ascorbic acid solid, preparing a reducing agent solution with a mass fraction of 15%, and then adding 300 g of polyvinyl pyrrolidone as a dispersant and 30 g of benzotriazole as a surfactant to the reducing agent solution, stirring evenly, to obtain a second solution; controlling the temperature of the first solution and the second solution at about 25°C.
[0056] Step S32. Add ammonia water to the second solution to adjust the pH value of the second solution to about 5, then add the second solution to the first solution under stirring and add the solution within 8 minutes. After adding, react for 10 minutes to obtain a silver powder suspension.
[0057] Step S33. Separate the silver powder suspension into solid and liquid, wash the separated solid with ultrapure water, and bake the washed solid in an oven at 60°C for 120 minutes to obtain the target product (ie, flower-shaped spherical silver powder A2).
[0058] Specifically, the scanning electron microscope image of the flower-shaped spherical silver powder A2 (eg Figure 3 As shown in the figure, the flower-shaped spherical silver powder A2 is a quasi-spherical silver powder with a special flower-shaped structure. In addition, by comparing the scanning electron microscope images of the flower-shaped spherical silver powder A2 with the scanning electron microscope images of the flower-shaped spherical silver powder A1, it can be seen that, that is, by comparing Figure 3 and Figure 2 It can be seen that in Example 2, the surfactant was changed, and the morphology and size of the flower-shaped spherical silver powder A2 obtained were significantly changed. For example, the flaky structure protruding on the surface of the flower-shaped spherical silver powder A2 became thinner. It can be seen that the morphology and size of the flower-shaped spherical silver powder can be effectively regulated by changing the surfactant, and the regulation method is simple.
[0059] Example 3
[0060] The preparation method of the flower-shaped spherical silver powder provided in Example 3 is basically the same as the preparation method of the flower-shaped spherical silver powder provided in Example 1. The difference between the two is that in Example 3, the temperature of the first solution and the second solution is controlled at about 45° C., instead of controlling the temperature of the first solution and the second solution at about 25° C. Accordingly, in Example 3, the specific process of the preparation method of the flower-shaped spherical silver powder can be as follows:
[0061] Step S41. preparing a first solution and a second solution, including: weighing 5 kg of silver nitrate solid, preparing a silver nitrate solution with a mass fraction of 5%, so as to obtain a first solution; weighing 2.6 kg of ascorbic acid solid, preparing a reducing agent solution with a mass fraction of 15%, and then adding 300 g of polyvinyl pyrrolidone as a dispersant and 30 g of sodium dodecylbenzene sulfonate as a surfactant to the reducing agent solution, stirring evenly, to obtain a second solution; controlling the temperature of the first solution and the second solution at about 45°C.
[0062] Step S42. Add ammonia water to the second solution to adjust the pH value of the second solution to about 5, then add the second solution to the first solution under stirring and add the solution within 8 minutes. After adding, react for 10 minutes to obtain a silver powder suspension.
[0063] Step S43. Separate the silver powder suspension into solid and liquid, wash the separated solid with ultrapure water, and bake the washed solid in an oven at 60° C. for 120 min to obtain the target product (ie, flower-shaped spherical silver powder A3).
[0064] Specifically, the scanning electron microscope image of the flower-shaped spherical silver powder A3 (eg Figure 4 As shown in the figure, the flower-shaped spherical silver powder A3 is a quasi-spherical silver powder with a special flower-shaped structure. In addition, by comparing the scanning electron microscope image of the flower-shaped spherical silver powder A3 with the scanning electron microscope image of the flower-shaped spherical silver powder A1, it can be seen that, that is, by comparing Figure 4 and Figure 2 It can be seen that in Example 3, the reaction temperature of the first solution and the second solution was changed, and the morphology and size of the flower-shaped spherical silver powder A3 obtained were significantly changed. For example, the protruding sheet structure on the surface of the flower-shaped spherical silver powder A3 became longer. It can be seen that the morphology and size of the flower-shaped spherical silver powder can be effectively controlled by changing the reaction temperature, and the control method is simple.
[0065] As can be seen from the above, the preparation method of the flower-shaped spherical silver powder provided in this embodiment is by preparing a first solution and a second solution, the first solution includes silver nitrate, the second solution includes a reducing agent, a dispersant and a surfactant, and then the pH value of the second solution is adjusted to a preset value, and then added to the first solution for reaction to obtain a silver powder suspension, the preset value is 3 to 7, and then the flower-shaped spherical silver powder is separated from the silver powder suspension. The flower-shaped spherical silver powder is a quasi-spherical silver powder with a flower-like structure, so that by introducing a surfactant, a flower-shaped spherical silver powder with a large specific surface area can be prepared. The preparation process is simple, and the morphology and size of the flower-shaped spherical silver powder can be effectively regulated by changing the amount and / or type of the surfactant, and the flower-shaped spherical silver powder can effectively avoid agglomeration and bridging effect, thereby ensuring good dispersibility and uniformity of the flower-shaped spherical silver powder, and has good application prospects in many fields such as conductive pastes and conductive coatings.
[0066] In order to better implement the method for preparing the flower-shaped spherical silver powder provided in the embodiment of the present application, the embodiment of the present application also provides a flower-shaped spherical silver powder (such as Figure 2 , Figure 3 or Figure 4 As shown), the flower-shaped spherical silver powder is prepared by the preparation method of the flower-shaped spherical silver powder provided by any of the above embodiments.
[0067] Specifically, the flower-shaped spherical silver powder has a rough surface and many protrusions, and thus has a large specific surface area and a high sintering activity, and has broad application prospects in the field of photovoltaic silver paste.
[0068] In some embodiments, the specific surface area of the flower-shaped spherical silver powder may be greater than or equal to 0.9 m 2 / g.
[0069] Furthermore, it should be noted that the flower-shaped spherical silver powder in the embodiment of the present application is prepared by the preparation method of the flower-shaped spherical silver powder provided by any of the above embodiments, and therefore has all the same beneficial effects, which will not be described in detail in this embodiment.
[0070] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0071] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing flower-shaped spherical silver powder, characterized in that: include: preparing a first solution and a second solution, wherein the first solution includes silver nitrate, and the second solution includes a reducing agent, a dispersant, and a surfactant; After adjusting the pH value of the second solution to a preset value, adding the second solution to the first solution for reaction to obtain a silver powder suspension, wherein the preset value is 3 to 7; Flower-shaped spherical silver powder is separated from the silver powder suspension, and the flower-shaped spherical silver powder is a quasi-spherical silver powder with a flower-shaped structure.
2. The preparation method according to claim 1, characterized in that: The mass concentration of the silver nitrate in the first solution is 5-25%, and the mass concentration of the reducing agent in the second solution is 10-20%; the ratio of the mass of the reducing agent in the second solution to the mass of the silver nitrate in the first solution is 50-60%; the ratio of the mass of the dispersant in the second solution to the mass of the silver nitrate in the first solution is 5-20%; the ratio of the mass of the surfactant in the second solution to the mass of the silver nitrate in the first solution is 0.5-5%.
3. The preparation method according to claim 1, characterized in that: The reducing agent includes at least one of glucose, ascorbic acid, hydrazine hydrate, hydrogen peroxide, formaldehyde and acetaldehyde; the dispersant includes at least one of polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene glycol, gum arabic, gelatin and Tween; the surfactant includes at least one of silane coupling agent, span, oleic acid, sodium dodecylbenzene sulfonate, methylbenzotriazole and benzotriazole.
4. The preparation method according to claim 3, characterized in that: The surfactant is sodium dodecylbenzene sulfonate or benzotriazole.
5. The preparation method according to claim 1, characterized in that: After adjusting the pH value of the second solution to a preset value, adding the second solution to the first solution for reaction to obtain a silver powder suspension comprises: The pH value of the second solution is adjusted to a preset value by adding a pH adjuster to the second solution, and then added to the first solution for reaction to obtain a silver powder suspension; the pH adjuster includes at least one of ammonia water, sodium hydroxide, sodium bicarbonate, oxalic acid, phosphoric acid, nitric acid, hydrochloric acid and sulfuric acid.
6. The preparation method according to claim 1, characterized in that: After adjusting the pH value of the second solution to a preset value, adding the second solution to the first solution for reaction to obtain a silver powder suspension comprises: After the pH value of the second solution is adjusted to a preset value, the second solution is added to the first solution under stirring for a preset addition time to react to obtain a silver powder suspension, wherein the preset addition time is 5 to 15 minutes.
7. The preparation method according to claim 1, characterized in that: After adjusting the pH value of the second solution to a preset value, adding the second solution to the first solution for reaction to obtain a silver powder suspension comprises: After the pH value of the second solution is adjusted to a preset value, it is added to the first solution to react at a preset reaction temperature to obtain a silver powder suspension, wherein the preset reaction temperature is 25-45°C.
8. The preparation method according to claim 1, characterized in that: The method of separating flower-shaped spherical silver powder from the silver powder suspension comprises: The silver powder suspension is separated into solid and liquid, the separated solid is washed, and the washed solid is dried at a drying temperature of 40 to 60° C. for 60 to 120 minutes to obtain flower-shaped spherical silver powder.
9. The preparation method according to claim 1, characterized in that: The specific surface area of the flower-shaped spherical silver powder is greater than or equal to 0.9 m 2 / g.
10. A flower-shaped spherical silver powder, characterized in that: The method is prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparing flower-like silver particles with controllable branch length through one-step method
CN109382524A
Silver powder with flower-shaped structure and preparation method thereof
CN114192769A
Preparation method of flower-shaped silver powder
CN115502408A
Preparation method of silver powder with adjustable sintering activity
CN116984621A
Preparation method of ball-flower-shaped silver powder with high specific surface area
CN117358941A
Cited By
Micron-sized flower-ball silver powder with adjustable surface roughness and preparation method of micron-sized flower-ball silver powder
CN121892702A