Preparation method of explosive composite board
By using rectangular wooden column support and explosive layer during the explosion composite process of medium-thick tube plates, gap-free bonding between the substrate and the composite plate is achieved, solving the problem of non-melting of intervals caused by the increase in composite layer thickness, and improving the product Quality and performance reduce production costs and risks.
Patent Information
- Application Number
- CN202411065100.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
During the explosion composite process of medium-thick tube plates, as the thickness of the composite layer increases, the difficulty of explosion increases, and the non-melting intervals lead to the impact of the quality of medium-thick tube plates. This problem is urgently needed to be solved to ensure its quality and performance.
The rectangular wooden column is used as the gap support, and the rock emulsified explosive and ammonium oil explosive are evenly arranged on the laminated plate. The interatomic metallurgical combination of the substrate and the laminated plate is achieved through explosion, and the gap-free bond is achieved by using the wooden column support and airflow discharge. .
The gapless explosion composite of medium and thick pipe plates is achieved, the fitting rate and shear strength are improved, the cost and explosion risk are reduced, and domestic low-risk mass production is achieved.
Smart Images

Figure CN118976975A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medium-thick tube sheet production, in particular to a method for preparing an explosive composite plate. Background Art
[0002] Medium and thick tube sheets include various types, such as titanium-steel tube sheets, stainless steel-steel tube sheets and nickel-steel tube sheets, which are widely used in various equipment, such as shell-and-tube heat exchangers, boilers, pressure vessels, steam turbines and large central air conditioners. These medium and thick tube sheets are mainly used in chemical containers, such as shell-and-tube heat exchangers, pressure vessels, boilers, condensers, central air conditioners, evaporators and seawater desalination devices, to support and fix the tubes. The metal material not only gives the medium and thick tube sheets strong rigidity, but also has excellent thermal conductivity.
[0003] However, during the explosive compounding process, as the thickness of the composite layer increases, the difficulty of the explosion increases gradually. The increase in the thickness of the composite layer leads to an increase in its weight, which requires thicker spacers to support it. However, the increase in the thickness of the spacers makes it difficult for the energy generated by the explosion to fully melt the spacers, resulting in the medium-thick tube sheet not melting during the explosive compounding process, which seriously affects the quality of the medium-thick tube sheet. Therefore, it is urgent to solve this problem to ensure the quality and performance of the medium-thick tube sheet. Summary of the invention
[0004] The purpose of the embodiment of the present invention is to provide a method for preparing an explosive composite plate, aiming to solve the technical problems mentioned in the background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing an explosive composite plate comprises the following steps:
[0007] S1: Select an area with solid and flat soil, lay a uniform layer of yellow sand, and level it as the foundation;
[0008] S2: Prepare the substrate and grind and polish it to ensure that its surface is smooth and free of impurities. Place the processed substrate on the leveled foundation and clean the excess yellow sand around the substrate.
[0009] S3: Select high-quality wood, accurately process it into rectangular wooden columns, and place them vertically and evenly on the edge of the substrate surface;
[0010] S4: Prepare the composite board and place it on the rectangular wooden column, ensuring that the composite board covers the rectangular wooden column evenly;
[0011] S5: evenly arranging the explosives on the composite plate to ensure that the explosives are evenly distributed to form an explosive layer;
[0012] S6: Place the detonator in the center of the composite plate and ensure that the detonator is firmly connected. Safely connect the fuse of the detonator to 50 meters away from the explosion site and set up a safe isolation zone. After the safe isolation zone is effectively established, ignite the fuse to cause the explosion.
[0013] Furthermore, the substrate is made of Q345R material, and the thickness of the substrate is 80 mm; the composite board is made of TA1 material, and the thickness of the composite board is 12 mm.
[0014] Furthermore, the dimensions of the rectangular wooden column are 28 mm in length, 14 mm in width, and 14 mm in height.
[0015] Further, in step S5, the surface of the composite plate is firstly subjected to a protective treatment, and then the rock emulsion explosive is evenly arranged;
[0016] Arrange a strip of ammonium oil-fuel mixture at the center of the surface of the composite plate, and the height of the ammonium oil-fuel mixture is flush with the height of the rock emulsion explosive to form an explosive layer;
[0017] The detonation point is set at the center of the ANFO mixture.
[0018] Furthermore, the detonation velocity of the rock emulsion explosive and the ammonium nitrate oil explosive is not less than 2500 mm / s.
[0019] Further, the ammonium oil-fuel mixture is arranged in a cylindrical shape, and the diameter of the ammonium oil-fuel mixture is 20 mm.
[0020] The invention provides a method for preparing an explosive composite plate, which has the following beneficial effects:
[0021] By using rectangular wooden columns as gap supports, it can not only bear the weight of the composite plate and the explosives on it, but also protect the bonding surface of the base plate and the composite plate from damage. Through this method of gap placement and arrangement of explosives, when detonated, the composite plate is accelerated to move toward the base plate under the action of the energy of the explosives. Since the wood gap will not melt, the airflow generated during the explosion will discharge the edge wood gap, so that the base plate and the composite plate can achieve good interatomic metallurgical bonding. This method realizes gapless explosive composite between medium and thick tube plates, and the properties such as bonding rate and shear strength meet the requirements. The produced medium and thick tube plates can be placed without gaps, which greatly saves costs and reduces the high risk caused by the non-melting of gaps during the explosion, achieving the goal of domestic low-risk mass production of explosive composite medium and thick tube plates. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The present invention is a schematic structural diagram of a foundation, a base plate, a rectangular square column, a composite plate, explosives and a detonator mentioned in a method for preparing an explosive composite plate.
[0023] In the figure: 1-foundation, 2-base plate, 3-rectangular wooden column, 4-composite plate, 5-explosive layer, 6-detonator. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0025] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0026] like Figure 1 As shown, a method for preparing an explosive composite plate provided by an embodiment of the present invention comprises the following steps:
[0027] S1: Select an area with solid and flat soil, lay a uniform layer of yellow sand, and level it as foundation 1;
[0028] S2: prepare a substrate 2, and grind and polish the substrate 2 to ensure that its surface is smooth and free of impurities, place the processed substrate 2 on the leveled foundation 1, and clean up excess yellow sand around the substrate 2. The substrate 2 is made of Q345R material, and the thickness of the substrate 2 is 80 mm;
[0029] Q345R is a low alloy steel mainly used for manufacturing pressure vessels. It has good mechanical properties and toughness and can withstand high temperature and high pressure environments. It has good tensile strength, yield strength and ductility and is widely used in the manufacture of boilers and pressure vessels, such as chemical plants, refineries and other equipment that require high temperature and high pressure resistance.
[0030] S3: Select high-quality wood and process it precisely into a rectangular wooden column 3, which is placed vertically and evenly on the edge of the surface of the substrate 2. The size of the rectangular wooden column 3 is 28 mm long, 14 mm wide and 14 mm high;
[0031] S4: prepare a composite board 4 and place the composite board 4 on the rectangular wooden column 3, ensuring that the composite board 4 evenly covers the rectangular wooden column 3, wherein the composite board 4 is made of TA1 material and has a thickness of 12 mm;
[0032] TA1 is a pure titanium material with extremely high corrosion resistance, excellent mechanical properties and high specific strength. TA1 can maintain stable performance even in high temperature environments and has good welding performance. It is widely used in aerospace, chemical, marine engineering and other fields, especially for equipment and components in corrosive environments.
[0033] S5: evenly arranging the explosives on the composite plate 4 to ensure that the explosives are evenly distributed to form an explosive layer 5;
[0034] In step S5, firstly, the surface of the composite plate 4 is protected, and then the rock emulsion explosive is evenly arranged;
[0035] A strip of ammonium oil-fuel mixture is arranged at the center of the surface of the composite plate 4, and the height of the ammonium oil-fuel mixture is flush with the height of the rock emulsion explosive to form an explosive layer 5;
[0036] The detonation point is set at the center of the ammonium nitrate oil explosive, the detonation velocity of the rock emulsion explosive and the ammonium nitrate oil explosive is not less than 2500mm / s, and the arrangement of the ammonium nitrate oil explosive is cylindrical, and the diameter of the ammonium nitrate oil explosive is 20mm;
[0037] S6: Place detonator 6 at the center of the composite plate 4 (i.e., the center of the ammonium nitrate explosive), and ensure that detonator 6 is firmly connected, safely connect the fuse of detonator 6 to 50 meters outside the explosion site, and set up a safe isolation zone. After the safe isolation zone is effectively established, ignite the fuse to cause the explosion.
[0038] In one embodiment of the present invention, in step S3, the number of rectangular wooden columns 3 can be adjusted according to the actual size of the base plate 2 and the composite board 4, and in principle, the larger the spacing between the rectangular wooden columns 3, the better, and the fewer the number of the rectangular wooden columns 3, the better, as long as it can support the composite board. The placement position of the rectangular wooden columns 3 should align the side with the largest force area with the detonation point position (the central area of the composite board) so that it can be subjected to more air wave impact at the moment of explosion, and then the rectangular wooden columns 3 can be blown out smoothly.
[0039] In step S6, after the fuse and detonator 6 are ignited, the explosive layer 5 produces a violent explosion reaction, and the composite plate 4 is accelerated to move toward the base plate 2 under the action of the explosive energy. Since the rectangular wooden column 3 will not melt, the airflow generated during the explosion will blow away the rectangular wooden column 3 at the edge position, so that the base plate 2 and the composite plate 4 can achieve good interatomic metallurgical bonding. As a supporting structure, the rectangular wooden column 3 can bear the weight of the composite plate 4 and the explosive thereon, and can protect the bonding surface of the base plate 2 and the composite plate 4 from damage.
[0040] In addition, since the rectangular wooden column 3 is made of wood material, it has the advantages of being easy to break, light in weight, and having no electrostatic adsorption. During the explosion, the wooden column 3 can be easily and completely broken and removed from between the base plate 2 and the composite plate 4.
[0041] Additionally, the composite plate 4 in the present method can also be made of copper, stainless steel or nickel, that is, the present method can be used for the production and preparation of medium-thick composite plates of titanium-steel tube plates, stainless steel-steel tube plates and nickel-steel tube plates.
[0042] The above method realizes gapless explosive composite between medium and thick tube sheets, and its performance such as bonding rate and shear strength can meet the standard ASTM B898-2016 "Technical Specifications for Active and Refractory Metal Composite Plates" and NB / T47002.3-2019 "Composite Plates for Pressure Vessels". Except for the detonation point (the detonation point can be placed at the perforation of the tube sheet to achieve a 99% bonding rate including the detonation point), the bonding rate can reach more than 99%, and the minimum shear strength τb ≥ 140Mpa. The produced TA1+Q345R tube sheet can be placed without gaps, which greatly saves costs and reduces the high risk caused by the non-melting of gaps during the explosion process, realizing the real domestic low-risk mass production of explosive composite medium and thick tube sheets.
[0043] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an explosive composite plate, characterized in that: The following steps are involved: S1: Select an area with solid and flat soil, lay a uniform layer of yellow sand, and level it as the foundation; S2: Prepare the substrate and grind and polish it to ensure that its surface is smooth and free of impurities. Place the processed substrate on the leveled foundation and clean the excess yellow sand around the substrate. S3: Select high-quality wood, accurately process it into rectangular wooden columns, and place them vertically and evenly on the edge of the substrate surface; S4: Prepare the composite board and place it on the rectangular wooden column, ensuring that the composite board covers the rectangular wooden column evenly; S5: evenly arranging the explosives on the composite plate to ensure that the explosives are evenly distributed to form an explosive layer; S6: Place the detonator in the center of the composite plate and ensure that the detonator is firmly connected. Safely connect the fuse of the detonator to 50 meters away from the explosion site and set up a safe isolation zone. After the safe isolation zone is effectively established, ignite the fuse to cause the explosion.
2. The method for preparing an explosive composite plate according to claim 1, characterized in that: The substrate is made of Q345R material, and the thickness of the substrate is 80 mm. The composite board is made of TA1 material, and the thickness of the composite board is 12 mm.
3. The method for preparing an explosive composite plate according to claim 1, characterized in that: The dimensions of the rectangular wooden column are 28 mm in length, 14 mm in width and 14 mm in height.
4. The method for preparing an explosive composite plate according to claim 1, characterized in that: In step S5, firstly, the surface of the composite plate is protected, and then the rock emulsion explosive is evenly arranged; Arrange a strip of ammonium oil-fuel mixture at the center of the surface of the composite plate, and the height of the ammonium oil-fuel mixture is flush with the height of the rock emulsion explosive to form an explosive layer; The detonation point is set at the center of the ANFO mixture.
5. The method for preparing an explosive composite plate according to claim 4, characterized in that: The detonation velocities of the rock emulsion explosive and the ammonium nitrate oil explosive are not less than 2500 mm / s.
6. The method for preparing an explosive composite plate according to claim 4, characterized in that: The ammonium oil-fuel mixture is arranged in a cylindrical shape, and the diameter of the ammonium oil-fuel mixture is 20 mm.