Noctilucent advertising material and preparation method thereof

By using a combination of forged aluminum foil layer, anti-aging agent, flame retardant and calcium fluoride-encapsulated rare earth luminescent materials in luminescent advertising materials, the problem of degradation of luminescent performance in extreme environments is solved, and the material is high stability is achieved and flame retardant, extending service life.

CN118977482APending Publication Date: 2024-11-19SHANGHAI HANKER PLASTICS
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411340608.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Rare earth luminous advertising materials have reduced luminous efficiency under extreme environmental conditions (such as extreme low temperatures or high temperatures), shortened luminous time, and may even experience luminous stops, lacking excellent weather resistance and high stability.

Method used

Using a luminous advertising material structure composed of aluminum foil layer, self-luminous layer and transparent release paper, the aluminum foil layer enhances strength and toughness through forging process, and the self-luminous layer is added with anti-aging agent, flame retardant and encapsulated rare earth luminous material, flame retardant The phosphorylated chitosan is combined with silver ions, and calcium fluoride wraps rare earth luminescent materials to isolate external harmful substances. The transparent release paper ensures uniform light.

Benefits of technology

It significantly improves the luminous stability, flame retardant performance and visual effect of luminous advertising materials, extends the service life, can maintain light effect under high and low temperature conditions, and enhances the weather resistance and ornamentality of the materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a noctilucent advertising material and a preparation method thereof, and relates to the technical field of advertising materials, the noctilucent advertising material comprises an aluminum foil layer, a self-luminous layer and a bottom layer from top to bottom; the aluminum foil layer is a forged aluminum foil, and the thickness of the aluminum foil layer is 0.1-0.2 mm; the bottom layer is transparent release paper, and the thickness of the bottom layer is 0.2-0.4 mm; the self-luminous layer is prepared from the following raw materials in percentage by weight: 18 to 22 percent of epoxy acrylate resin, 2 to 4 percent of an anti-aging agent, 2 to 4 percent of a flatting agent, 0.5 to 1.5 percent of a de-foaming agent, 3.5 to 4.5 percent of a flame retardant, 27 to 41 percent of ethyl acetate and 30 to 40 percent of a coated rare earth luminous material; and the thickness of the self-luminous layer is 0.1 to 0.5 mm. The noctilucent advertising material provided by the invention has excellent weather resistance and flame retardance, stable luminous efficiency and long service cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of advertising material technology, and in particular to a luminous advertising material and a preparation method thereof. Background Art

[0002] Luminous advertising materials have emerged in the advertising market in recent years. This type of material, with its unique self-light absorption and self-luminous properties, provides new possibilities for advertising display. It not only provides warning and direction in the dark, but is also favored by advertisers for its unique visual effects. At present, luminous advertising materials are mainly used in scenes such as bridge billboards, lamp post flags, road column flags, construction site fence advertisements, building construction frame advertisements, light boxes, advertising stickers, and vehicle body advertisements. In the road traffic safety products market, such as temporary construction signs, road signs, crash barrels, road cones, and vehicle body reflective signs, they are also widely used.

[0003] In the relevant technology, rare earth elements show excellent luminous effects in luminous materials due to their unique electronic structure and optical properties. At present, the application of rare earth luminous advertising materials in the advertising field is gradually increasing, especially at night or in a dimly lit environment, its luminous effect can attract people's attention and enhance the publicity effect of advertising.

[0004] Although rare earth luminous advertising materials have shown great potential in the field of advertising and signage with their unique luminous properties and environmental advantages, their application under extreme environmental conditions still faces technical challenges that cannot be ignored. Under extremely low or high temperature conditions, rare earth luminous advertising materials will experience reduced luminous efficiency, shortened luminous time, and may even stop luminescence. Therefore, there is an urgent need to provide a luminous advertising material with excellent weather resistance and high stability. Summary of the invention

[0005] In order to provide a luminous advertising material with excellent weather resistance and high stability, the present application provides a luminous advertising material and a preparation method thereof.

[0006] The luminous advertising material provided in this application adopts the following technical solution: A luminous advertising material comprises, from top to bottom, an aluminum foil layer, a self-luminous layer, and a bottom layer; the aluminum foil layer is a forged aluminum foil with a thickness of 0.1-0.2 mm; the bottom layer is a transparent release paper with a thickness of 0.2-0.4 mm; the raw materials of the self-luminous layer include, by weight percentage, 18-22% of epoxy acrylate resin, 2-4% of an antioxidant, 2-4% of a leveling agent, 0.5-1.5% of a defoaming agent, 3.5-4.5% of a flame retardant, 27-41% of ethyl acetate, and 30-40% of an encapsulated rare earth luminescent material; the thickness of the self-luminous layer is 0.1-0.5 mm.

[0007] By adopting the above technical scheme, the aluminum foil layer adopts a forging process and has high strength and toughness, which can effectively protect the inner layer of self-luminous material from external physical damage. At the same time, the addition of antioxidants also enhances the anti-aging properties of the material and extends its service life. The encapsulated rare earth luminescent material used in the self-luminous coating can effectively isolate harmful substances in the external environment, such as oxygen, moisture, etc., thereby protecting the rare earth luminescent material from erosion, further improving its weather resistance, and improving the luminous stability of the luminous advertising material; the use of flame retardants significantly enhances the flame retardancy of the luminous advertising material; the bottom layer adopts transparent release paper, which not only ensures the overall lightness of the material, but also allows the light of the self-luminous layer to penetrate evenly and softly, improving the visual effect and ornamental value.

[0008] Preferably, the raw materials of the self-luminous layer include 20% epoxy acrylate resin, 3% antioxidant, 3% leveling agent, 1% defoaming agent, 4% flame retardant, 34% ethyl acetate, and 35% encapsulated rare earth by weight percentage.

[0009] Preferably, the flame retardant is prepared from the following raw materials in parts by weight: 1-2 parts of phosphorylated chitosan, 3-6 parts of acetic acid, 100-150 parts of water, and 0.004-0.008 parts of silver nitrate aqueous solution.

[0010] By adopting the above technical scheme, the flame retardant obtained by compounding phosphorylated chitosan and silver ions can significantly improve the flame retardant properties of luminous advertising materials. The phosphorus element can promote the formation of a carbon layer during combustion, isolate oxygen and heat, and thus play a flame retardant role. Chitosan and its phosphorylated products also have good biocompatibility and degradability. Phosphorylation modification may further improve its physical properties and enhance the strength, toughness and stability of the luminous advertising materials.

[0011] Preferably, the phosphorylated chitosan is prepared from the following raw materials in parts by weight: 1-2 parts chitosan powder, 10-20 parts Urea, 2-4 parts of orthophosphoric acid, 19-38 parts of N,N-dimethylformamide.

[0012] Preferably, the encapsulated rare earth luminescent material raw material is prepared from the following raw materials in parts by weight: 30-40 parts of rare earth luminescent material, 3.5-4.5 parts of calcium chloride, 2.2-3 parts of ammonium fluoride, and 15-25 parts of anhydrous ethanol; the rare earth luminescent material is a composite yttrium oxide / terbium material.

[0013] By adopting the above technical scheme, calcium fluoride prepared by calcium chloride and ammonium fluoride is used to wrap the rare earth luminescent material, which can effectively isolate harmful substances in the external environment, such as oxygen, moisture, etc., thereby protecting the rare earth luminescent material from corrosion and extending its service life; calcium fluoride has a low refractive index and a wide band gap, and its light transmittance range can be from the vacuum ultraviolet to the infrared region. Therefore, the use of a calcium fluoride coating layer will not have a negative impact on the luminescent properties of the rare earth luminescent material, and can also enhance or regulate its luminescent properties.

[0014] Preferably, the composite yttrium oxide / terbium material is prepared from the following raw materials in parts by volume: 2.5-3 parts of yttrium nitrate solution, 0.8-1.2 parts of terbium nitrate solution, and 8-14 parts of distilled water.

[0015] The present application also provides a method for preparing luminous advertising materials, which adopts the following technical solution: A method for preparing a luminous advertising material comprises the following steps: S1. The epoxy acrylate resin, flame retardant, rare earth luminescent material, ethyl acetate are mixed and stirred evenly, and after cooling, an antioxidant, a leveling agent, a defoaming agent are added, and after stirring, a self-luminous coating is obtained; S2. Apply the self-luminous paint on the surface of the forged aluminum foil, and then attach a transparent release paper. After drying, bond them together to obtain the luminous advertising material.

[0016] Preferably, the method for preparing the flame retardant comprises the following steps: Add chitosan powder, urea and orthophosphoric acid into N,N-dimethylformamide and stir to dissolve, and stir to react for 1-2 hours under a protective atmosphere. After the reaction is completed, cool and filter, and wash and dry the separated solid product to obtain phosphorylated chitosan; Phosphorylated chitosan is added to a mixed solution of acetic acid and water, stirred until completely dissolved, and then an aqueous silver nitrate solution is added to react for 20-28 hours. After the reaction is completed, the pH of the solution is adjusted to neutral to obtain a neutral solution, and the neutral solution is dried at 75-85°C for 20-28 hours to obtain a flame retardant.

[0017] Preferably, the method for preparing the encapsulated rare earth luminescent material comprises the following steps: Add calcium chloride and ammonium fluoride to anhydrous ethanol, stir and dissolve, and stir in a water bath at 70-80°C for 15-25 minutes; then add rare earth luminescent material, stir in a water bath at 70-80°C for 2-3 hours, ultrasonically disperse for 15-20 minutes, and then vacuum filter. The solid product is dried at 60-70°C for 2-3 hours. After washing and drying, an encapsulated rare earth luminescent material is obtained.

[0018] Preferably, the method for preparing the rare earth luminescent material comprises the following steps:.

[0019] After the yttrium nitrate solution, terbium nitrate solution and distilled water are mixed evenly, they are continuously stirred and the pH value of the solution is adjusted to 8-9. The mixture is reacted at a temperature of 160-200°C for 10-14 hours. After the reaction is completed, the mixture is cooled and filtered. The obtained solid product is washed, dried at 60-70°C for 5-7 hours, and then calcined at 1000-1200°C for 1-2 hours to obtain a rare earth luminescent material.

[0020] In summary, the present application includes at least one of the following beneficial technical effects: 1. By adopting the above technical scheme, the aluminum foil layer adopts the forging process, has high strength and toughness, and can effectively protect the inner layer of self-luminous material from external physical damage. The self-luminous coating adopts the encapsulated rare earth luminescent material, which can effectively isolate harmful substances in the external environment, such as oxygen, moisture, etc., thereby protecting the rare earth luminescent material from erosion, further improving its weather resistance, and improving the luminous stability of the luminous advertising material; the use of flame retardants significantly enhances the flame retardancy of the luminous advertising material; the bottom layer adopts transparent release paper, which not only ensures the overall lightness of the material, but also allows the light of the self-luminous layer to be evenly and softly transmitted, improving the visual effect and ornamental value; 2. By adopting the above technical scheme, the flame retardant obtained by compounding phosphorylated chitosan and silver ions can significantly improve the flame retardant properties of luminous advertising materials. Phosphorus can promote the formation of a carbon layer during combustion, isolate oxygen and heat, and thus play a flame retardant role. Chitosan and its phosphorylated products also have good biocompatibility and degradability. Phosphorylation modification may further improve its physical properties and enhance the strength, toughness and stability of luminous advertising materials. 3. By adopting the above technical solution, the calcium fluoride prepared by calcium chloride and ammonium fluoride is used to wrap the rare earth luminescent material, which can effectively isolate harmful substances in the external environment, such as oxygen, moisture, etc., thereby protecting the rare earth luminescent material from corrosion and extending its service life; calcium fluoride has a low refractive index and a wide band gap, and its light transmittance range can be from vacuum ultraviolet to infrared regions. Therefore, the use of a calcium fluoride coating layer will not have a negative impact on the luminescent properties of the rare earth luminescent material, and can also enhance or regulate its luminescent properties. DETAILED DESCRIPTION

[0021] The present application is further described in detail below with reference to the embodiments.

[0022] The chemical reagents used in the embodiments and comparative examples provided by the present invention are all commercially available products, and their brands and manufacturers are as follows: Chitosan powder, Hebei Clavier Biotechnology Co., Ltd.; Epoxy acrylate resin, Guangdong Yunxing Biotechnology Co., Ltd.; Antiaging agent, Panhua Chemical (Shanghai) Co., Ltd., KY-405; Leveling agent, Guangzhou Qianguang Trading Co., Ltd., BYK-354 from Germany; Defoaming agent, Shanghai McLean Biochemical Technology Co., Ltd., silicone defoaming agent, non-ionic, viscosity 160-200mpas.

[0023] Preparation Example Preparation Example 1 Preparation of flame retardant Preparation Example 1.1 T1. Add 1g chitosan powder, 10g urea and 2g orthophosphoric acid to 19g N,N-dimethylformamide and stir to dissolve. Under nitrogen protection, stir and react at 150°C for 1h. After the reaction, cool and filter. Wash the separated solid product with distilled water and dry it in a forced air drying oven at 60°C for 24h to obtain phosphorylated chitosan. T2. Add 1 g of phosphorylated chitosan obtained from T1 to a mixed solution of 3 g of acetic acid and 100 g of water, stir until completely dissolved, then add 0.004 g of 1 g / L silver nitrate aqueous solution to react for 20 hours. After the reaction, adjust the pH of the solution to neutral by adding sodium hydroxide solution to obtain a neutral solution. Dry the neutral solution at 75°C for 20 hours to obtain a flame retardant.

[0024] Preparation Example 1.2 T1. Add 1.5g chitosan powder, 15g urea and 3g orthophosphoric acid to 28.5g N,N-dimethylformamide and stir to dissolve. Under nitrogen protection, stir and react at 155°C for 1.5h. After the reaction, cool and filter. Wash the separated solid product with distilled water and dry it in a forced air drying oven at 65°C for 26h to obtain phosphorylated chitosan. T2. Add 1.5 g of phosphorylated chitosan obtained from T1 to a mixed solution of 4.5 g of acetic acid and 125 g of water, stir until completely dissolved, then add 0.006 g of 1 g / L silver nitrate aqueous solution to react for 24 hours. After the reaction, adjust the pH of the solution to neutral by adding sodium hydroxide solution to obtain a neutral solution. Dry the neutral solution at 80°C for 24 hours to obtain a flame retardant.

[0025] Preparation Example 1.3 T1. Add 2g chitosan powder, 20g urea and 4g orthophosphoric acid to 38g N,N-dimethylformamide and stir to dissolve. Under nitrogen protection, stir and react at 160°C for 2h. After the reaction, cool and filter. Wash the separated solid product with distilled water and dry it in a blast drying oven at 70°C for 28h to obtain phosphorylated chitosan. T2. Add 2 g of phosphorylated chitosan obtained from T1 to a mixed solution of 6 g of acetic acid and 150 g of water, stir until completely dissolved, then add 0.008 g of 1 g / L silver nitrate aqueous solution to react for 28 hours. After the reaction, adjust the pH of the solution to neutral by adding sodium hydroxide solution to obtain a neutral solution. Dry the neutral solution at 85°C for 28 hours to obtain a flame retardant.

[0026] Preparation Example 2 Encapsulated Rare Earth Luminescent Material Preparation Example 2.1 T1. After 2.5 mL of 0.2 mol / L yttrium nitrate aqueous solution, 0.8 mL of 0.2 mol / L terbium nitrate aqueous solution and 8 mL of distilled water were mixed evenly, stirred continuously, and the pH of the solution was adjusted to 8 by dropping ammonia water. The mixture was reacted at 160°C for 10 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. The obtained solid product was washed 3 times each with distilled water and anhydrous ethanol in a centrifuge, dried in an oven at 60°C for 5 h, and then calcined in a muffle furnace at 1000°C for 2 h to obtain a rare earth luminescent material; T2. Add 3.5g of calcium chloride and 2.2g of ammonium fluoride to 15g of anhydrous ethanol, stir to dissolve, and stir in a water bath at 70°C for 15 minutes; then add 30g of the rare earth luminescent material prepared by T1, stir in a water bath at 70°C for 2 hours, ultrasonically disperse at 1000kHz for 15 minutes, and then vacuum filter. Dry the solid product at 60°C for 3 hours, wash it three times with anhydrous ethanol, and after drying, obtain the encapsulated rare earth luminescent material.

[0027] Preparation Example 2.2 T1. Mix 2.8 mL of 0.2 mol / L yttrium nitrate aqueous solution, 1.0 mL of 0.2 mol / L terbium nitrate aqueous solution, and 10 mL of distilled water, stir continuously, and adjust the pH of the solution to 8.5 by adding ammonia water. React at 180 ° C for 12 hours. After the reaction is completed, cool to room temperature and filter. Wash the obtained solid product with distilled water and anhydrous ethanol in a centrifuge for 3 times each, dry it in an oven at 65 ° C for 6 hours, and then heat it in a muffle furnace at 1100 ° C. Calcinate for 1.5 hours to obtain a rare earth luminescent material; T2. Add 4g of calcium chloride and 2.6g of ammonium fluoride to 20g of anhydrous ethanol, stir to dissolve, and stir in a water bath at 75°C for 20 minutes; then add 35g of the rare earth luminescent material prepared by T1, stir in a water bath at 75°C for 2.5 hours, ultrasonically disperse at 1100kHz for 18 minutes, and then vacuum filter, dry the solid product at 65°C for 2.5 hours, wash 3 times with anhydrous ethanol, and after drying, obtain an encapsulated rare earth luminescent material.

[0028] Preparation Example 2.3 T1. After 3 mL of 0.2 mol / L yttrium nitrate aqueous solution, 1.2 mL of 0.2 mol / L terbium nitrate aqueous solution, and 14 mL of distilled water were mixed evenly, stirred continuously, and the pH of the solution was adjusted to 9 by dropping ammonia water. The mixture was reacted at 200°C for 14 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. The obtained solid product was washed 3 times each with distilled water and anhydrous ethanol in a centrifuge, dried in an oven at 70°C for 7 h, and then calcined in a muffle furnace at 1200°C for 1 h to obtain a rare earth luminescent material; T2. Add 4.5g of calcium chloride and 3g of ammonium fluoride to 25g of anhydrous ethanol, stir to dissolve, and stir in a water bath at 80°C for 25min; then add 40g of the rare earth luminescent material prepared by T1, stir in a water bath at 80°C for 3h, ultrasonically disperse at 1200kHz for 20min, and then vacuum filter. Dry the solid product at 70°C for 3h, wash it 3 times with anhydrous ethanol, and after drying, obtain the encapsulated rare earth luminescent material. Example

[0029] Example 1 S1. 20g of epoxy acrylate resin, 4g of the flame retardant prepared in Preparation Example 1.1, 35g of the encapsulated rare earth luminescent material prepared in Preparation Example 2.1, and 34g of ethyl acetate were mixed and stirred at 55°C for 4h, and after cooling for 1.5h, 3g of antioxidant, 3g of leveling agent, and 1g of defoaming agent were added, and stirred at 900rpm for 50min to obtain a self-luminous coating; S2. The self-luminous coating is applied on the surface of the forged aluminum foil with a thickness of 0.15 mm, and the coating thickness is 0.3 mm. Then, a transparent release paper with a thickness of 0.3 mm is attached. After drying and bonding, the luminous advertising material is obtained.

[0030] Example 2 S1. 20g of epoxy acrylate resin, 4g of the flame retardant prepared in Preparation Example 1.1, 35g of the encapsulated rare earth luminescent material prepared in Preparation Example 2.1, and 34g of ethyl acetate were mixed and stirred at 60°C for 3h, and after cooling for 2h, 3g of antioxidant, 3g of leveling agent, and 1g of defoaming agent were added. After stirring at 1000rpm for 30min, a self-luminous coating was obtained; S2. The self-luminous coating is applied on the surface of the forged aluminum foil with a thickness of 0.1 mm, and then a transparent release paper with a thickness of 0.2 mm is attached. After drying and bonding, the luminous advertising material is obtained.

[0031] Example 3 S1. 20g of epoxy acrylate resin, 4g of the flame retardant prepared in Preparation Example 1.1, 35g of the encapsulated rare earth luminescent material prepared in Preparation Example 2.1, and 34g of ethyl acetate were mixed and stirred at 65°C for 2.5h, and after cooling for 3h, 3g of antioxidant, 3g of leveling agent, and 1g of defoaming agent were added. After stirring at 1100rpm for 25min, a self-luminous coating was obtained; S2. Apply the self-luminous paint on the surface of the forged aluminum foil with a thickness of 0.2 mm, with a coating thickness of 0.5 mm, and then attach a transparent release paper with a thickness of 0.4 mm. After drying and bonding, the luminous advertising material is obtained.

[0032] Example 4 S1. 18 g of epoxy acrylate resin, 4.5 g of the flame retardant prepared in Preparation Example 1.1, 30 g of the encapsulated rare earth luminescent material prepared in Preparation Example 2.1, and 41 g of ethyl acetate were mixed and stirred at 55 ° C for 4 h, and after cooling for 1.5 h, 2 g of antioxidant, 4 g of leveling agent, and 0.5 g of defoaming agent were added, and stirred at 900 rpm for 50 min to obtain a self-luminous coating; S2. The self-luminous coating is applied on the surface of the forged aluminum foil with a thickness of 0.15 mm, and the coating thickness is 0.3 mm. Then, a transparent release paper with a thickness of 0.3 mm is attached. After drying and bonding, the luminous advertising material is obtained.

[0033] Example 5 S1. 22g of epoxy acrylate resin, 3.5g of the flame retardant prepared in Preparation Example 1.1, 40g of the encapsulated rare earth luminescent material prepared in Preparation Example 2.1, and 27g of ethyl acetate were mixed and stirred at 55°C for 4h, and after cooling for 1.5h, 4g of antioxidant, 2g of leveling agent, and 1.5g of defoaming agent were added, and stirred at 900rpm for 50min to obtain a self-luminous coating; S2. The self-luminous coating is applied on the surface of the forged aluminum foil with a thickness of 0.15 mm, and the coating thickness is 0.3 mm. Then, a transparent release paper with a thickness of 0.3 mm is attached. After drying and bonding, the luminous advertising material is obtained.

[0034] Example 6 The difference between Example 6 and Example 1 is that the flame retardant used in the preparation of the self-luminous coating in S1 of Example 6 comes from Preparation Example 1.2.

[0035] Example 7 The difference between Example 7 and Example 1 is that the flame retardant used in the preparation of the self-luminous coating in S1 of Example 7 comes from Preparation Example 1.3.

[0036] Example 8 The difference between Example 8 and Example 1 is that the encapsulated rare earth luminescent material used in the preparation of the self-luminous coating in S1 of Example 8 comes from Preparation Example 2.2.

[0037] Example 9 The difference between Example 9 and Example 1 is that the encapsulated rare earth luminescent material used in the preparation of the self-luminous coating in S1 of Example 9 comes from Preparation Example 2.3.

[0038] Comparative Example Comparative Example 1 S1. 16g of epoxy acrylate resin, 4.8g of the flame retardant prepared in Preparation Example 1.1, 25g of the encapsulated rare earth luminescent material prepared in Preparation Example 2.1, and 48g of ethyl acetate were mixed and stirred at 55°C for 4h, and after cooling for 1.5h, 1g of antioxidant, 5g of leveling agent, and 0.2g of defoaming agent were added, and stirred at 900rpm for 50min to obtain a self-luminous coating; S2. The self-luminous coating is applied on the surface of the forged aluminum foil with a thickness of 0.15 mm, and the coating thickness is 0.3 mm. Then, a transparent release paper with a thickness of 0.3 mm is attached. After drying and bonding, the luminous advertising material is obtained.

[0039] Comparative Example 2 S1. 24g of epoxy acrylate resin, 3g of the flame retardant prepared in Preparation Example 1.1, 45g of the encapsulated rare earth luminescent material prepared in Preparation Example 2.1, and 20g of ethyl acetate were mixed and stirred at 55°C for 4h, and after cooling for 1.5h, 5g of antioxidant, 1g of leveling agent, and 2g of defoaming agent were added, and stirred at 900rpm for 50min to obtain a self-luminous coating; S2. The self-luminous coating is applied on the surface of the forged aluminum foil with a thickness of 0.15 mm, and the coating thickness is 0.3 mm. Then, a transparent release paper with a thickness of 0.3 mm is attached. After drying and bonding, the luminous advertising material is obtained.

[0040] Performance testing 1. The limiting oxygen index of the luminous advertising materials obtained in Examples 1-9 and Comparative Examples 1-2 was tested using GB / T 2406.2-2009 "Determination of Combustion Behavior by Oxygen Index Method for Plastics". The results are shown in Table 1. 2. The luminous advertising materials obtained in Examples 1-9 and Comparative Examples 1-2 were placed in an environment of 200°C and baked for 100 hours, and then taken out and naturally cooled. If the materials did not lose their luminous efficacy, the test result was judged to be "qualified", otherwise it was "unqualified"; 3. Freeze the luminous advertising materials obtained in Examples 1-9 and Comparative Examples 1-2 at -50°C for 1 hour, then take them out and quickly place them at 50°C for 0.5 hour, and repeat this cycle 50 times; if the material does not lose its luminous effect, the test result is judged as "qualified", otherwise it is "unqualified" The specific test results are as follows: Table 1 Performance test results Limiting oxygen index % High temperature resistance test Low temperature resistance test Example 1 34 qualified qualified Example 2 37 qualified qualified Example 3 35 qualified qualified Example 4 34 qualified qualified Example 5 32 qualified qualified Example 6 35 qualified qualified Example 7 33 qualified qualified Example 8 35 qualified qualified Example 9 33 qualified qualified Comparative Example 1 26 Failure Failure Comparative Example 2 24 Failure Failure It can be seen from the test results in Table 1 that the luminous advertising material provided by the present application has a relatively high limiting oxygen index, indicating that the material has good flame retardant properties; and can withstand high and low temperature tests, indicating that the material has strong weather resistance.

[0041] It can be seen from the test results of Comparative Examples 1-2 that the self-luminous layer of the present application can obtain flame-retardant and weather-resistant luminous advertising materials when the weight percentage of the raw materials is 18-22% epoxy acrylate resin, 2-4% antioxidant, 2-4% leveling agent, 0.5-1.5% defoaming agent, 3.5-4.5% flame retardant, 27-41% ethyl acetate, and 30-40% encapsulated rare earth luminescent material, and the preferred weight percentage of the raw materials for the self-luminous layer is 20% epoxy acrylate resin, 3% antioxidant, 3% leveling agent, 1% defoaming agent, 4% flame retardant, 34% ethyl acetate, and 35% encapsulated rare earth.

[0042] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A luminous advertising material, characterized in that: The luminous advertising material includes an aluminum foil layer, a self-luminous layer, and a bottom layer from top to bottom; the aluminum foil layer is a forged aluminum foil; the bottom layer is a transparent release paper; the raw materials of the self-luminous layer include, by weight percentage, 18-22% epoxy acrylate resin, 2-4% antioxidant, 2-4% leveling agent, 0.5-1.5% defoaming agent, 3.5-4.5% flame retardant, 27-41% ethyl acetate, and 30-40% encapsulated rare earth luminescent material.

2. The luminous advertising material according to claim 1, characterized in that: The raw materials of the self-luminous layer include 20% epoxy acrylate resin, 3% antioxidant, 3% leveling agent, 1% defoaming agent, 4% flame retardant, 34% ethyl acetate, and 35% encapsulated rare earth luminescent material by weight percentage.

3. The luminous advertising material according to claim 1, characterized in that: The flame retardant is prepared from the following raw materials in parts by weight: 1-2 parts of phosphorylated chitosan, 3-6 parts of acetic acid, 100-150 parts of water, and 0.004-0.008 parts of silver nitrate aqueous solution.

4. The luminous advertising material according to claim 3, characterized in that: The phosphorylated chitosan is prepared from the following raw materials in parts by weight: 1-2 parts of chitosan powder, 10-20 parts of urea, 2-4 parts of orthophosphoric acid, and 19-38 parts of N,N-dimethylformamide.

5. The luminous advertising material according to claim 1, characterized in that: The encapsulated rare earth luminescent material raw material is prepared from the following raw materials in parts by weight: 30-40 parts of rare earth luminescent material, 3.5-4.5 parts of calcium chloride, 2.2-3 parts of ammonium fluoride, and 15-25 parts of anhydrous ethanol; the rare earth luminescent material is a composite yttrium oxide / terbium material.

6. The luminous advertising material according to claim 5, characterized in that: The composite yttrium oxide / terbium material is prepared from the following raw materials in parts by volume: 2.5-3 parts of 0.2 mol / L yttrium nitrate solution, 0.8-1.2 parts of 0.2 mol / L terbium nitrate solution, and 8-14 parts of distilled water.

7. A method for preparing a luminous advertising material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. The epoxy acrylate resin, flame retardant, rare earth luminescent material, ethyl acetate are mixed and stirred evenly, and after cooling, an antioxidant, a leveling agent, a defoaming agent are added, and after stirring, a self-luminous coating is obtained; S2. Apply the self-luminous paint on the surface of the forged aluminum foil, and then attach a transparent release paper, and after bonding, the luminous advertising material is obtained.

8. The method for preparing a luminous advertising material according to claim 7, characterized in that: The method for preparing the flame retardant comprises the following steps: Add chitosan powder, urea and orthophosphoric acid into N,N-dimethylformamide and stir to dissolve, and stir to react for 1-2 hours under a protective atmosphere. After the reaction is completed, cool and filter, and wash and dry the separated solid product to obtain phosphorylated chitosan; Phosphorylated chitosan is added to a mixed solution of acetic acid and water, stirred until completely dissolved, and then an aqueous silver nitrate solution is added to react for 20-28 hours. After the reaction is completed, the pH of the solution is adjusted to neutral to obtain a neutral solution, and the neutral solution is dried at 75-85°C for 20-28 hours to obtain a flame retardant.

9. The method for preparing a luminous advertising material according to claim 7, characterized in that: The method for preparing the encapsulated rare earth luminescent material comprises the following steps: Add calcium chloride and ammonium fluoride to anhydrous ethanol, stir and dissolve, and stir in a water bath at 60-68°C for 15-25 minutes; then add rare earth luminescent material, stir in a water bath at 60-68°C for 2-3 hours, ultrasonically disperse for 15-20 minutes, and then vacuum filter. The solid product is dried at 60-70°C for 2-3 hours. After washing and drying, an encapsulated rare earth luminescent material is obtained.

10. The method for preparing a luminous advertising material according to claim 9, characterized in that: The method for preparing the rare earth luminescent material comprises the following steps: After the yttrium nitrate solution, terbium nitrate solution and distilled water are mixed evenly, they are continuously stirred and the pH value of the solution is adjusted to 8-9. The mixture is reacted at a temperature of 160-200°C for 10-14 hours. After the reaction is completed, the mixture is cooled and filtered. The obtained solid product is washed, dried at 60-70°C for 5-7 hours, and then calcined at 1000-1200°C for 1-2 hours to obtain a rare earth luminescent material.

Citation Information

Patent Citations

  • Method for preparing terbium-doped yttria green-light luminescent powder

    CN101560389A

  • Luminescent material and preparation method and application thereof

    CN102807866A

  • Self-luminous advertising printing coating

    CN104804589A

  • Printing paint for self-luminous advertisements and preparation method thereof

    CN107141926A

  • Noctilucent advertising paper and preparation method thereof

    CN109203615A