Rare earth-containing phosphite as well as preparation method, application and composition thereof

By reacting rare earth phosphite with inorganic aluminum salt and combining with aluminum diethylphosphinate, a nylon composition with high flame retardant properties and fluidity is formed, which solves the problem of insufficient flame retardant properties of existing polymer materials. , suitable for aerospace and electronic devices and other fields.

CN118978134AActive Publication Date: 2024-11-19BAOTOU RESEARCH INSTITUTE OF RARE EARTHS +1

Patent Information

Application Number
CN202411064826.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The flame retardant properties of existing polymer materials are insufficient, especially the water resistance and temperature resistance of rare earth oxides in hydration reactions, which will affect their application in aerospace and electronic devices.

Method used

By reacting rare earth phosphite with inorganic aluminum salt in water, a rare earth phosphite containing salt with improved flame retardant properties of nylon was prepared, and combined with aluminum diethyl phosphinate to form a composition with good flame retardant effect. .

Benefits of technology

It significantly improves the flame retardant performance, fluidity and impact strength of nylon, enhances its stability in high temperature and high humidity environments, and is suitable for aerospace and electronic devices and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978134A_ABST
    Figure CN118978134A_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth-containing phosphite as well as a preparation method, application and a composition thereof. The preparation method provided by the invention comprises the following step: reacting rare earth phosphite with inorganic aluminum salt in the presence of water to obtain the phosphite containing rare earth. The rare earth-containing phosphite prepared by the method can effectively improve the flame retardance of nylon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a rare earth-containing phosphite and a preparation method, use and composition thereof. Background Art

[0002] Polymer materials have the advantages of low density, high strength, good toughness, and good insulation performance, and are widely used in aerospace, electronic devices, construction and other fields. However, the flame retardant properties of some polymer materials need to be improved, and flame retardants need to be added when used. The application of rare earth elements in polymer flame retardant materials has received widespread attention.

[0003] CN106315536A discloses a method for preparing rare earth phosphate, wherein a precipitant is added to a suspension of rare earth carbonate or rare earth oxide under constant stirring at room temperature until the pH is less than or equal to 5; stirring is continued for 5 to 30 minutes, and the pH is observed to no longer increase, which means that the reaction end point has been reached; if the pH rises to more than 2 during stirring, the precipitant is continued to be added until the pH is less than or equal to 5, stirring and observing until the reaction end point; precipitation, dehydration, and washing are performed to obtain rare earth phosphate. The method is used to prepare rare earth phosphate.

[0004] CN11483991A discloses a method for preparing lanthanum phosphite, which comprises the following steps: adding an appropriate amount of water to a reaction kettle, heating and stirring the water, and maintaining the water temperature at 20-35°C; sequentially adding lanthanum oxide and a catalyst to the water, and then continuing to stir evenly and maintaining the water temperature at 30-35°C, and reacting water, lanthanum oxide and the catalyst to generate a hydration reactant; adding the hydration reactant to the reaction kettle of the hydration reactant, continuously dripping phosphorous acid thereto, maintaining the temperature in the hydration reaction kettle at 40-80°C until the dripping is completed, and heat-retaining the reaction for 2-5 hours to obtain a white phosphite rare earth product; cooling the phosphite rare earth product to room temperature, and then filtering it in a filter, placing the filtered material in an oven, maintaining the oven temperature at 100-150°C, and crushing the dried material to obtain a finished lanthanum phosphite. The method uses rare earth oxide as a raw material, and the product obtained contains hydroxyl groups, and the water resistance and temperature resistance of the product need to be improved. Summary of the invention

[0005] In view of this, one object of the present invention is to provide a method for preparing a rare earth phosphite. The rare earth phosphite prepared by the method of the present invention can effectively improve the flame retardancy of nylon. Furthermore, the nylon composition containing the rare earth phosphite prepared by the method of the present invention has good fluidity. Furthermore, the nylon composition containing the rare earth phosphite prepared by the method of the present invention has high impact strength and corrosiveness. Another object of the present invention is to provide a rare earth phosphite. Another object of the present invention is to provide a use of a rare earth phosphite. Another object of the present invention is to provide a flame retardant composition. Another object of the present invention is to provide a nylon composition.

[0006] The above purpose is achieved through the following technical solutions.

[0007] In one aspect, the present invention provides a method for preparing a rare earth phosphite, comprising the following steps:

[0008] The rare earth phosphite and the inorganic aluminum salt are reacted in the presence of water to obtain the rare earth-containing phosphite.

[0009] According to the preparation method of the present invention, preferably, the rare earth element in the rare earth phosphite is selected from one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium;

[0010] The inorganic aluminum salt is selected from one or more of aluminum sulfate, aluminum nitrate, aluminum chloride, and chloroacetate;

[0011] The molar ratio of the aluminum element in the rare earth phosphite and the inorganic aluminum salt is (0.2-3.5):2.

[0012] According to the preparation method of the present invention, preferably, the rare earth phosphite is mixed with water, and then an inorganic aluminum salt is added;

[0013] The reaction temperature is 50-90°C and the reaction time is 1-7h.

[0014] According to the preparation method of the present invention, preferably, it further comprises the step of adding a phosphorous acid solution dropwise into a mixed solution containing water and a rare earth carbonate to obtain a rare earth phosphite.

[0015] According to the preparation method of the present invention, preferably, the molar ratio of rare earth carbonate to phosphorous acid is 1:(1.5-4).

[0016] On the other hand, the present invention provides a rare earth-containing phosphite, which is obtained by the above preparation method.

[0017] In another aspect, the present invention provides a use of a rare earth phosphite in improving the flame retardancy and / or fluidity of a polymer.

[0018] In another aspect, the present invention provides a flame retardant composition, comprising the rare earth phosphite and aluminum diethylphosphinate.

[0019] In yet another aspect, the present invention provides a nylon composition comprising nylon and the flame retardant composition.

[0020] According to the nylon composition of the present invention, preferably, the nylon composition further comprises one or more of an antioxidant, a lubricant, a masterbatch and glass fiber.

[0021] The rare earth phosphite prepared by the method of the present invention can effectively improve the flame retardancy of nylon. Furthermore, the nylon composition containing the rare earth phosphite prepared by the method of the present invention has good fluidity. Furthermore, the nylon composition containing the rare earth phosphite prepared by the method of the present invention has high impact strength and corrosiveness. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the infrared spectrum of the lanthanum cerium phosphite obtained in Preparation Example 1.

[0023] Figure 2 This is the infrared spectrum of the lanthanum cerium phosphite obtained in Preparation Example 2.

[0024] Figure 3 This is the infrared spectrum of the lanthanum cerium phosphite obtained in Preparation Example 3.

[0025] Figure 4 The XRD patterns of the lanthanum cerium phosphite obtained in Preparation Examples 1 to 3 are shown in FIG.

[0026] Figure 5 The XRD diagrams of the rare earth-containing phosphites obtained in Examples 1-2 and the lanthanum cerium phosphite obtained in Preparation Example 2 are shown.

[0027] Figures 6-7 These are SEM images of different locations of the lanthanum cerium phosphite obtained in Preparation Example 2.

[0028] Figures 8 to 11 These are SEM images of different locations of the rare earth phosphite obtained in Example 1.

[0029] Figures 12 to 15 These are SEM images of different locations of the rare earth phosphite obtained in Example 2. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0031] <Preparation method of rare earth phosphite>

[0032] The preparation method of the rare earth-containing phosphite of the present invention comprises the following steps: reacting the rare earth phosphite and an inorganic aluminum salt in the presence of water to obtain the rare earth-containing phosphite.

[0033] The rare earth element in the rare earth phosphite is selected from one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium. Preferably, the rare earth element in the rare earth phosphite is selected from one or more of lanthanum and cerium. More preferably, the rare earth phosphite is lanthanum cerium phosphite.

[0034] The inorganic aluminum salt can be a soluble inorganic aluminum salt or a sparingly soluble inorganic aluminum salt. Preferably, the inorganic aluminum salt is selected from one or more of aluminum sulfate, aluminum nitrate, aluminum chloride, and aluminum acetate. More preferably, the inorganic aluminum salt is aluminum sulfate.

[0035] The molar ratio of the aluminum element in the rare earth phosphite and the inorganic aluminum salt is (0.2-3.5):2; preferably (0.5-3):2. In some embodiments, the molar ratio of the aluminum element in the rare earth phosphite and the inorganic aluminum salt is (0.8-1.2):2. In other embodiments, the molar ratio of the aluminum element in the rare earth phosphite and the inorganic aluminum salt is (1.8-2.2):2.

[0036] According to one embodiment of the present invention, the rare earth phosphite is lanthanum cerium phosphite. The inorganic aluminum salt is aluminum sulfate. The mass ratio of lanthanum cerium phosphite to aluminum sulfate is (100-500):257; preferably (150-450):257; more preferably (200-400):257. The mass of aluminum sulfate is calculated as aluminum sulfate 18hydrate.

[0037] The reaction temperature may be 50 to 90°C; preferably 60 to 80°C; more preferably 70 to 75°C.

[0038] The reaction time may be 1 to 7 hours, preferably 2 to 6 hours, and more preferably 3 to 5 hours.

[0039] The mass ratio of water to rare earth phosphite may be (1-6):1; preferably (2-5):1; more preferably (3-4.5):1.

[0040] According to one embodiment of the present invention, rare earth phosphite and water are mixed and heated to 50-90° C., preferably 60-80° C., more preferably 70-75° C., and then an inorganic aluminum salt is added.

[0041] In some embodiments, the method further comprises the following steps: cooling the product obtained by the reaction of the rare earth phosphite and the inorganic aluminum salt, filtering to obtain a solid product, washing the solid product, and drying at 90 to 150° C., preferably 100 to 130° C., to obtain a rare earth phosphite.

[0042] In certain embodiments, the method further comprises the step of adding a phosphorous acid solution dropwise into a mixed solution containing water and a rare earth carbonate to obtain a rare earth phosphite.

[0043] The rare earth element in the rare earth carbonate is selected from one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium. Preferably, the rare earth element in the rare earth carbonate is selected from one or more of lanthanum and cerium. More preferably, the rare earth carbonate is lanthanum cerium carbonate. The content of lanthanum carbonate in lanthanum cerium carbonate can be 60-85wt%; more preferably 65-80wt%; more preferably 70-85wt%. The content of cerium carbonate in lanthanum cerium carbonate can be 15-40wt%; preferably 20-35wt%; more preferably 25-30wt%.

[0044] The molar ratio of rare earth carbonate to phosphorous acid may be 1:(1.5-4); preferably 1:(2-3.5); more preferably 1:(2.4-2.6).

[0045] The temperature of the mixed solution may be 60 to 110°C, preferably 70 to 100°C, and more preferably 80 to 90°C.

[0046] The concentration of the phosphorous acid solution may be 30 to 70 wt %, preferably 40 to 60 wt %, and more preferably 50 to 55 wt %. The phosphorous acid solution includes phosphorous acid and water.

[0047] The mass ratio of water to rare earth carbonate in the mixed solution can be (2-5):1; preferably (3-4):1.

[0048] After the phosphorous acid solution is added dropwise, the phosphorous acid and the rare earth carbonate are allowed to react for 1 to 8 hours, preferably 3 to 7 hours, and more preferably 5 to 6 hours.

[0049] In some embodiments, the method may further include the following steps: filtering the reaction product obtained by the reaction of phosphorous acid and rare earth carbonate to obtain a filter cake. The filter cake is washed with water at 50 to 90° C., preferably 60 to 80° C., and the washed filter cake is dried at 120 to 170° C., preferably 140 to 160° C., to obtain rare earth phosphite.

[0050] <Rare earth-containing phosphites and their uses>

[0051] The rare earth-containing phosphite of the present invention is prepared by the above method. The rare earth-containing phosphite can improve the flame retardant properties of the polymer; and after being added to the polymer, the composition has good fluidity. Therefore, the present invention also provides the use of the rare earth-containing phosphite in improving the flame retardant properties and / or fluidity of the polymer. In certain embodiments, the rare earth-containing phosphite is used to improve the flame retardant properties of the polymer. In other embodiments, the rare earth-containing phosphite is used to improve the fluidity of the polymer.

[0052] The polymer is preferably nylon. Nylon can be selected from one or more of PA6, PA66, PA11, and PA12. According to one embodiment of the present invention, nylon is a mixture of PA6 and PA66. The mass ratio of PA6 to PA66 can be 10:(20-60); preferably 10:(30-50); more preferably 10:(35-45).

[0053] <Flame Retardant Composition>

[0054] The flame retardant composition of the present invention comprises the rare earth-containing phosphite and aluminum diethylphosphinate. The present invention finds that compounding the rare earth-containing phosphite with aluminum diethylphosphinate has a better flame retardant effect.

[0055] The amount of rare earth phosphite used can be 1 to 6 parts by weight, preferably 2 to 5 parts by weight, and more preferably 3 to 4 parts by weight.

[0056] The amount of aluminum diethylphosphinate used may be 8 to 18 parts by weight, preferably 10 to 16 parts by weight, and more preferably 12 to 15 parts by weight.

[0057] <Nylon composition>

[0058] The nylon composition of the present invention comprises nylon and the flame retardant composition. In certain embodiments, the nylon composition may further comprise one or more of an antioxidant, a lubricant, a masterbatch and glass fiber. The flame retardant composition is specifically as described above and will not be described in detail herein.

[0059] The amount of nylon can be 30 to 70 parts by weight, preferably 40 to 60 parts by weight, and more preferably 50 to 55 parts by weight. Nylon can be selected from one or more of PA6, PA66, PA11, and PA12. According to one embodiment of the present invention, nylon is a mixture of PA6 and PA66. The mass ratio of PA6 to PA66 can be 10:(20 to 60), preferably 10:(30 to 50), and more preferably 10:(35 to 45).

[0060] The amount of the antioxidant can be 0.1 to 1.5 parts by weight, preferably 0.3 to 1 parts by weight, and more preferably 0.5 to 0.8 parts by weight. The antioxidant can be a mixture of antioxidant 1098 and antioxidant 608. The mass ratio of antioxidant 1098 to antioxidant 608 can be 2:(1 to 5), and preferably 2:(3 to 4).

[0061] The amount of the lubricant can be 0.1 to 1 part by weight, preferably 0.2 to 0.8 part by weight, and more preferably 0.3 to 0.5 part by weight. The lubricant can be wax powder. According to one embodiment of the present invention, the lubricant is AC540A produced by Honeywell.

[0062] The amount of the masterbatch can be 0.3 to 3 parts by weight, preferably 0.5 to 2 parts by weight, and more preferably 1 to 1.5 parts by weight. A black masterbatch is preferred. According to one embodiment of the present invention, the masterbatch is PA3785 produced by Cabot Corporation of the United States.

[0063] The amount of glass fiber used may be 10 to 50 parts by weight, preferably 20 to 40 parts by weight, and more preferably 30 to 35 parts by weight.

[0064] The nylon composition of the present invention can be prepared by the following method: extruding the raw material through a twin-screw extruder to obtain a molding material, cooling the molding material, and then granulating to obtain the nylon composition.

[0065] Here are the raw materials:

[0066] The PA6 grade is 2400J and was purchased from Hangzhou Juheshun New Materials Co., Ltd.

[0067] The PA66 grade is EPR24, which was purchased from Pingdingshan Shenma Engineering Plastics Co., Ltd.

[0068] The glass fiber grade is ECS301UW, which was purchased from Chongqing International Composite Materials Co., Ltd.

[0069] OP1400 is a complex of aluminum diethylphosphinate and aluminum phosphite, purchased from Clariant Chemicals.

[0070] ADP-33 is aluminum diethylphosphinate, purchased from Qingdao Oupure New Materials Co., Ltd.

[0071] Lubricant AC540A was purchased from Honeywell.

[0072] Black masterbatch: brand PA3785, purchased from Cabot Corporation, USA.

[0073] Antioxidant 608 was purchased from QiTi Technology Co., Ltd.

[0074] Here is the test method:

[0075] If the following test methods require processing into test pieces, the nylon composition shall be dried and then processed into test pieces on an injection molding machine at 280°C, unless otherwise specified.

[0076] UL94: HB grade is evaluated by horizontal burning test, and V0-V2 grade is evaluated by 500W (125mm) vertical burning test.

[0077] Notched impact strength: tested using the method specified in ISO 179-1.

[0078] Preparation Examples 1 to 3

[0079] Add water to lanthanum cerium carbonate (lanthanum carbonate content is 75wt%, cerium carbonate content is 25wt%), stir evenly and heat to 90°C to obtain a mixed solution. In the mixed solution, the mass ratio of lanthanum cerium carbonate to water is 1:3. Mix phosphorous acid and water to obtain a phosphorous acid solution with a concentration of 50wt%.

[0080] The phosphorous acid solution was added dropwise to the mixed solution. After the phosphorous acid solution was added dropwise, the mixture was reacted for 6 hours to obtain a reaction product. The reaction product was filtered while hot to obtain a filter cake. The filter cake was washed with 70°C water and dried at 150°C to obtain lanthanum cerium phosphite.

[0081] The molar ratio of lanthanum cerium carbonate and phosphorous acid is shown in Table 1. The 1 wt% thermal weight loss temperature of lanthanum cerium phosphite is obtained according to the TG curve, and the obtained results are shown in Table 1.

[0082] Figures 1 to 3 The infrared spectra of the cerium lanthanum phosphite obtained in Preparation Examples 1 to 3 are shown in Figure 1. -1 The left and right sides are the peaks of pH, 800~1160cm -1 The left and right sides are the absorption peaks of PO and P=O; 3600cm -1 The peaks on the left and right are OH peaks.

[0083] Figure 4 The XRD patterns of lanthanum cerium phosphite obtained in Preparation Examples 1 to 3 are shown in FIG. Figure 4 It can be seen that the XRD diffraction peaks of the lanthanum cerium phosphite obtained in Preparation Examples 1 to 3 are basically consistent.

[0084] Table 1

[0085]

[0086] Example 1

[0087] 800 g of water was added to 200 g of lanthanum cerium phosphite obtained by the method of Preparation Example 3, and the mixture was stirred and dispersed and heated to 70° C. Then 257 g of aluminum sulfate 18hydrate was added and reacted at 70° C. for 5 h to obtain a product. The product was cooled and filtered to obtain a solid product. The solid product was washed and dried at 120° C. to obtain a rare earth-containing phosphite.

[0088] The TG curve shows that the thermal weight loss temperature of 1 wt% rare earth phosphite obtained in this example is 287.6°C.

[0089] Example 2

[0090] Except that the amount of lanthanum cerium phosphite used is 400g, the rest is the same as Example 1.

[0091] The TG curve shows that the thermal weight loss temperature of 1 wt% rare earth phosphite obtained in this example is 286.9°C.

[0092] Figure 5 The XRD patterns of the rare earth-containing phosphites obtained in Examples 1 and 2 and the cerium lanthanum phosphite obtained in Preparation Example 2 are shown in FIG. Figure 5 It can be seen that when aluminum sulfate is added to lanthanum cerium phosphite, the XRD diffraction peak of the obtained rare earth phosphite is basically consistent with the XRD diffraction peak of lanthanum cerium phosphite, indicating that the physical phase of lanthanum cerium phosphite has not changed, but the addition of aluminum sulfate can make the diffraction peak of lanthanum cerium phosphite higher and improve the crystallinity.

[0093] Figures 6-7 These are SEM images of different locations of the lanthanum cerium phosphite obtained in Preparation Example 2. Figures 8 to 11 These are SEM images of different locations of the rare earth phosphite obtained in Example 1. Figures 12 to 15 The following are SEM images of different positions of the rare earth phosphite obtained in Example 2. Figures 6 to 15 It can be seen that the lanthanum cerium phosphite obtained in Preparation Example 2 is dispersed in rhombus flakes or arranged and condensed into irregular blocks; the rare earth-containing phosphites obtained in Examples 1 to 2 are blocky grains in the shape of columns or oblique rhombuses, and the grain surface is not smooth with small grain protrusions.

[0094] Examples 3 to 4 and Comparative Examples 1 to 4

[0095] 40.2 parts by weight of PA66 (nylon 66) and 10 parts by weight of PA6 (nylon 6) were placed in a twin-screw extruder (model: KTS35 / 44D); the materials shown in Table 2 were mixed and then added to the twin-screw extruder from the first side feed port at 260°C; 30 parts by weight of glass fiber were added to the twin-screw extruder through the second side feed port; and the molded material was extruded through the twin-screw extruder to obtain the molded material. The molded material was cooled in a water bath and then granulated to obtain a nylon composition.

[0096] The properties of the nylon composition are shown in Table 2.

[0097] Table 2

[0098]

[0099] Note: Each set of UL94 tests is conducted five times. A*X means that the results of grade A are X times out of five tests.

[0100] Corrosion test

[0101] PA66 and PA6 are placed in a twin-screw extruder (model: KTS35 / 44D); a die head of the twin-screw extruder is provided with a mass of m 1 a brass block; a flame retardant (selected from one or more of phosphite, OP1400, ADP-33 and aluminum phosphite), an antioxidant 1098, an antioxidant 608, AC540A and a black masterbatch are mixed, and then added to a twin-screw extruder from a first side feed port at 260° C.; glass fiber is added to the twin-screw extruder through a second side feed port; and a molding material is obtained by extruding through the twin-screw extruder. The molding material is cooled in a water bath and then granulated.

[0102] The total weight of the raw materials (PA66, PA6, flame retardant, antioxidant 1098, antioxidant 608, AC540A, black masterbatch and glass fiber) is 25 kg.

[0103] Measure the mass of the brass block on the die head after granulation, recorded as m 2 According to the formula (m 1 -m 2 ) / m 1 The loss amount of the brass block was calculated, and the corrosiveness of the composition was judged based on the loss amount of the brass block.

[0104] The selection and proportion of each raw material are shown in Table 3, and the corrosiveness is shown in Table 3.

[0105] Table 3

[0106]

[0107] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for preparing a rare earth phosphite, characterized in that: The steps include: The rare earth phosphite and the inorganic aluminum salt are reacted in the presence of water to obtain the rare earth-containing phosphite.

2. The preparation method according to claim 1, characterized in that: The rare earth element in the rare earth phosphite is selected from one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium; The inorganic aluminum salt is selected from one or more of aluminum sulfate, aluminum nitrate, aluminum chloride, and chloroacetate; The molar ratio of the aluminum element in the rare earth phosphite and the inorganic aluminum salt is (0.2-3.5):

2.

3. The preparation method according to claim 1, characterized in that: Mixing a rare earth phosphite with water and then adding an inorganic aluminum salt; The reaction temperature is 50-90°C and the reaction time is 1-7h.

4. The preparation method according to claim 1, characterized in that: The following steps are also included: The phosphorous acid solution is added dropwise to a mixed solution containing water and rare earth carbonate to obtain rare earth phosphite.

5. The preparation method according to claim 4, characterized in that: The molar ratio of rare earth carbonate to phosphorous acid is 1:(1.5-4).

6. A rare earth phosphite, characterized in that: The rare earth-containing phosphite is obtained by the preparation method according to any one of claims 1 to 5.

7. Use of the rare earth phosphite according to claim 6 in improving the flame retardant properties and / or fluidity of a polymer.

8. A flame retardant composition, characterized in that The flame retardant composition comprises the rare earth phosphite as claimed in claim 6 and aluminum diethylphosphinate.

9. A nylon composition, characterized in that: The nylon composition comprises nylon and the flame retardant composition according to claim 8.

10. The nylon composition according to claim 9, characterized in that The nylon composition further comprises one or more of an antioxidant, a lubricant, a masterbatch and glass fiber.

Citation Information

Patent Citations

  • High-thermal-conductivity flame-retarding nylon composite and its preparation method

    CN107652672A

  • Halogen-free solid flame retardant mixture and use thereof

    CN109796628A

  • Preparation method of lanthanum phosphite

    CN111483991A

  • Dialkyl phosphinic acid-aluminum phosphite composite salt and preparation method and application thereof

    CN112876736A

  • Phosphate material, flame-retardant additive composition, flame retardant composition, halogen-free flame-retardant material, preparation method and application

    CN116812894A

Cited By

  • Functional plastic and preparation method thereof

    CN121779912A

  • A functional plastic and a method for producing the same

    CN122898128A