Method for preparing hard carbon and sodium ion battery from mask and application
Through the sulfonation of the masks in a sulfonation of sulfuric acid and the pre-carbonization treatment of the staged heating and pre-carbonization treatment under an argon environment, the problem of complete decomposition of PP waste after heating was solved, and high-efficiency hard carbon materials for sodium ion batteries were prepared, which enhanced its commercial value. and application prospects.
Patent Information
- Application Number
- CN202411316418.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art is difficult to effectively convert the waste of disposable medical masks into functional carbon materials with commercial value, especially because meltblown cloth (PP) is completely decomposed after heating, resulting in residues and high specific surface area during its carbonization process. The problem.
By immersing the sheared mask in concentrated sulfuric acid, and then pre-carbonizing it in sections under argon environment, hard carbon is prepared by using different temperatures, combined with sulfonation crosslinking technology, the thermal stability of the PP molecular chain is improved and inhibited The release of gaseous small molecules reduces the residual carbon rate.
The conversion of PP waste into value-added hard carbon is achieved and used in the negative electrode material of sodium ion battery, which significantly improves the electrochemical storage capacity and cycle stability, and provides new application prospects.
Smart Images

Figure CN118978147A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery preparation, and in particular to a method for preparing hard carbon and sodium ion batteries from a mask and application thereof. Background Art
[0002] Disposable medical masks have become a necessity in people's daily lives, but the disposal of used masks faces daunting challenges. It is of great significance to convert such waste into commercially viable value-added products through recycling.
[0003] Generally speaking, masks are mainly composed of meltblown polypropylene (PP), which is the second most common general-purpose plastic. Since PP is a carbon-rich polymer with a carbon content of up to 85%, converting PP into functional carbon materials will greatly increase the recycling market value of its waste.
[0004] However, PP completely decomposes without residue upon heating in an inert environment. This characteristic of the PP molecule poses a severe challenge to the preparation of PP-based functional carbon materials. Therefore, the development of efficient PP carbonization recycling methods is crucial and has good development prospects and application areas. Summary of the Invention
[0005] The purpose of the present invention is to provide a method and application of preparing hard carbon and sodium ion batteries from masks, aiming to provide an efficient PP carbonization recovery method.
[0006] To achieve the above objectives, in a first aspect, the present invention provides a method for preparing hard carbon for a mask, comprising the following steps:
[0007] Cut the mask into small pieces and immerse them in concentrated sulfuric acid, then sulfonate them in an oil bath at a constant temperature to obtain a sulfide material;
[0008] The sulfide material is diluted with clean water until the pH reaches neutral, and then dried to obtain black sulfide;
[0009] Pre-carbonizing the black sulfide in a tube furnace under an argon environment by heating the black sulfide in stages to obtain a pre-carbonized product;
[0010] The pre-carbonized products were divided into three groups and carbonized at different temperatures in a vertical high-temperature experimental furnace in an argon atmosphere to obtain hard carbon.
[0011] The constant temperature sulfonation conditions are as follows: an oil bath at 180° C., stirring at a rate of 600 rpm, and a constant temperature sulfonation time of 3 hours.
[0012] The specific method of diluting the sulfide material with clean water until the pH reaches neutral and then drying it to obtain black sulfide is as follows:
[0013] Diluting the sulfide material with clean water, extracting the supernatant after precipitation, and leaving the precipitate;
[0014] Repeatedly diluting the precipitate with clean water and testing the pH until the pH of the precipitate reaches neutral to obtain a central precipitate;
[0015] The central precipitate was dried at a constant temperature of 100° C. for 10 hours using a constant temperature blower dryer to obtain a black sulfide.
[0016] Among them, the segmented heating pre-carbonization is divided into three stages. In the first stage, the temperature is raised to 300°C at a heating rate of 2°C / min and kept warm for 2 hours. In the second stage, the temperature is raised to 500°C at a heating rate of 2°C / min and kept warm for 2 hours. In the third stage, the temperature is raised to 900°C at a heating rate of 2°C / min and kept warm for 2 hours.
[0017] In the second aspect, the present invention also provides an application of hard carbon in preparing sodium ion batteries, which is applied to the method for preparing hard carbon for a mask described in the first aspect above, comprising using the prepared hard carbon to prepare an electrode sheet, assembling the electrode sheet, button battery shell, button battery shrapnel, button battery gasket, glass fiber, commercial button battery sodium sheet and NaPF6 electrolyte into a button battery in a glove box, and conducting electrochemical constant current charge and discharge tests at room temperature using a Xinwei battery system.
[0018] The present invention discloses a method for preparing hard carbon for a mask, comprising the following steps: cutting the mask into small pieces and immersing the pieces in concentrated sulfuric acid, followed by constant-temperature sulfonation in an oil bath to obtain a sulfide material; diluting the sulfide material with clean water until the pH value reaches neutral, and then drying the piece to obtain a black sulfide; placing the black sulfide in a tubular furnace under an argon environment and performing segmented heating for pre-carbonization to obtain a pre-carbonized product; dividing the pre-carbonized product into three groups, and carbonizing the pieces at different temperatures in a vertical high-temperature experimental furnace under an argon atmosphere to obtain hard carbon. In this method for preparing hard carbon, sulfonation and crosslinking effectively improve the thermal stability of PP molecular chains, thereby inhibiting the rapid release of gaseous small molecules during the carbonization process. The residual carbon rate is 52.65%, and the specific surface area of the hard carbon is reduced. The method is a direct sulfonation strategy, which can convert PP-based meltblown cloth waste into value-added hard carbon and has good application prospects in sodium ion battery negative electrode materials, thereby opening up new possibilities for various potential applications of other polyolefins. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0020] Figure 1 Schematic diagram of the conversion of waste masks into hard carbon materials (CM-x).
[0021] Figure 2 It is a schematic diagram of the thermogravimetric (TGA) curve under N2 atmosphere.
[0022] Figure 3 This is a schematic diagram of the scanning electron microscope (SEM) of the sulfonated sample and its high-temperature carbonization product at 10,000 times magnification.
[0023] Figure 4 (a) is a schematic diagram of the X-ray diffraction (XRD) pattern, (b) is a schematic diagram of the Raman spectrum (RAMAN), and (c) is a schematic diagram of the pore size distribution curve of CM-x.
[0024] Figure 5 Schematic diagram of high-resolution transmission electron microscopy with different CM-x samples and different resolutions.
[0025] Figure 6 (a) is a schematic diagram of X-ray photoelectron spectroscopy (XPS), and (b)-(d) are C1s peak diagrams of CM-x.
[0026] Figure 7 (a)-(c) CM-x at 0.0001V s -1 Cyclic voltammetry (CV) curves at scan rates, and the corresponding (d)-(f) constant current charge-discharge curves at 0.1C for the initial three cycles, (g) CV comparison curve of the second cycle of CM-x, (h) second charge curve of CM-x, (i) comparison of the capacity of CM-x in the slope region and plateau region based on the second charge curve.
[0027] Figure 8 (a) Cycling performance at 0.1C, (b) cycling performance at 0.5C, (c) cycling performance at 1C, (d) rate capability at different current rates, (e) electrochemical impedance spectroscopy (EIS) of the CM-x electrode, (f) the initial three constant current charge-discharge curves of the full cell at 0.1C, and (g) cycling performance at 0.1C.
[0028] Figure 9 The present invention is a flow chart of a method for preparing hard carbon for a mask. DETAILED DESCRIPTION
[0029] The following describes embodiments of the present invention in detail, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and are not to be construed as limiting the present invention.
[0030] See also Figures 1 to 8 In a first aspect, the present invention provides a method for preparing hard carbon for a mask, comprising the following steps:
[0031] S1 cuts the mask into small pieces and immerses them in concentrated sulfuric acid, then sulfonates them in an oil bath at a constant temperature to obtain a sulfide material;
[0032] In an embodiment of the present invention, the microstructure of the meltblown cloth in the mask was observed to be in the form of a molecular chain under a scanning electron microscope (SEM). The meltblown cloth was cut into small pieces and then completely immersed in concentrated sulfuric acid. The pieces were then sulfonated at a constant temperature of 180°C in an oil bath at a stirring rate of 600 rpm for 3 hours.
[0033] S2 dilutes the sulfide material with clean water until the pH reaches neutral, and then dries it to obtain black sulfide;
[0034] In the embodiment of the present invention, a large amount of clean water is used to dilute it, and after precipitation, the supernatant is extracted to retain the precipitate, and the precipitate is repeatedly diluted until its pH reaches neutral, and then dried in a constant temperature blower dryer at 100° C. for 10 hours to obtain a black sulfonated product.
[0035] Specific method:
[0036] S21 dilutes the sulfide material with clean water, extracts the supernatant after precipitation, and retains the precipitate;
[0037] S22 repeatedly diluting the precipitate with clean water and detecting the pH until the pH of the precipitate reaches neutral, thereby obtaining a central precipitate;
[0038] S23 uses a constant temperature blower dryer to dry the central precipitate at 100° C. for 10 hours to obtain a black sulfide.
[0039] S3 pre-carbonizing the black sulfide in a tube furnace under an argon environment by heating the black sulfide in stages to obtain a pre-carbonized product;
[0040] In an embodiment of the present invention, the obtained sulfonated product is placed in a tube furnace under an argon environment at a heating rate of 2°C / min to 300°C and kept warm for 2 hours, then heated to 500°C at a heating rate of 2°C / min and kept warm for 2 hours, and finally heated to 900°C at a heating rate of 2°C / min and kept warm for 2 hours to obtain a pre-carbonized product.
[0041] S4: dividing the pre-carbonized products into three groups, and carbonizing them at different temperatures in a vertical high-temperature experimental furnace in an argon atmosphere to obtain hard carbon.
[0042] In an embodiment of the present invention: the pre-carbonized products are divided into three groups, and the temperature is raised to 1050°C at a heating rate of 5°C / min in a vertical high-temperature experimental furnace in an argon atmosphere, and then kept at 1200°C, 1300°C, and 1400°C at a heating rate of 3°C / min for 2 hours respectively, to obtain hard carbon prepared at different high-temperature carbonization temperatures.
[0043] In a second aspect, the present invention further provides an application of hard carbon in preparing sodium ion batteries, which is applied to the method for preparing hard carbon for a mask described in the first aspect.
[0044] The method includes using the prepared hard carbon to prepare an electrode sheet, assembling the electrode sheet, a button battery shell, a button battery shrapnel, a button battery gasket, glass fiber, a commercial button battery sodium sheet and NaPF6 electrolyte into a button battery in a glove box, and conducting an electrochemical constant current charge and discharge test at room temperature using a Xinwei battery system.
[0045] In order to better understand the present technical solution, the following examples are provided for further explanation:
[0046] The experiment changes the temperature as above to obtain
[0047] The hard carbons prepared at different high temperature carbonization temperatures were obtained by keeping the temperature at 1200°C, 1300°C and 1400°C for 2 hours.
[0048] Example 1
[0049] Microstructure analysis
[0050] Figure 1 A general diagram of the transformation of meltblown fabric into amorphous carbon (CM-x) is shown. The uncarbonized PP-based mask is first sulfonated in concentrated sulfuric acid to form a highly stable carbon precursor with abundant oxygen functional groups serving as crosslinking sites. A subsequent high-temperature carbonization process yields amorphous hard carbon with high disorder, large interlayer spacing, and low specific surface area.
[0051] TGA curve ( Figure 2 ) showed that the untreated mask completely decomposed at approximately 482°C, while the sulfonated mask retained residual products even at pyrolysis temperatures, indicating that sulfonation crosslinking can significantly alter the decomposition behavior and improve the thermal stability of the mask-derived carbon precursor. Notably, with increasing sulfonation time, the primary weight loss of SM-x gradually shifted to lower temperatures. With increasing sulfonation time, the carbon yield of SM-x gradually increased from 46.09% for SM-2h to 52.65% for SM-3h.
[0052] By SEM( Figure 3) The morphology of the sulfonated samples and their high-temperature carbonization products were observed at a magnification of 10,000 times. The fibrous structure of the meltblown cloth was completely destroyed, and it can be clearly observed that the morphology of the samples after high-temperature carbonization was irregular and contained voids.
[0053] The XRD patterns and Raman spectra were analyzed to study the effect of carbonization temperature on the microstructure of CM-x. Figure 4 a shows that all CM-x have two broad diffraction peaks centered at 23° and 44° in the XRD pattern, corresponding to the typical (002) and (100) crystal planes in the hard carbon structure, respectively. This indicates that the interlayer spacing increases due to the introduction of more oxygen functional groups. The increased interlayer spacing is beneficial to the Na + storage and transportation, thereby comprehensively improving the electrochemical storage capacity of carbon electrodes.
[0054] Figure 4 b is the Raman spectrum of CM-x, where the G band is 1600 cm -1 The E2g vibration mode corresponding to the sp2 carbon atom in-plane stretching vibration is 1350 cm -1 The D band at [C] is associated with the Alg vibration caused by the breathing vibration of sp2 carbon defects in the hexagonal carbon ring and at the edge. Defects or disorder in the carbon structure can be quantitatively evaluated by estimating the integrated intensity ratio of the G and D bands (IG / ID). The IG / ID value of CM-x remains essentially unchanged with increasing carbonization temperature. This is likely because at higher carbonization temperatures, other impurity elements in the PP molecule essentially disappear, leaving only the hard carbon structural elements.
[0055] The specific surface area of CM-x was studied, such as Figure 4 c. This indicates that during the high-temperature carbonization process of the cross-linked precursor structure, as the carbonization temperature increases, small molecules such as H2O, SO2, and CO2 are released, resulting in an increase in the specific surface area. However, when the temperature reaches 1400°C, the carbonization temperature may be too high, resulting in excessive carbonization of the carbon atoms in the carbon precursor.
[0056] Figure 5 AI shows high-resolution transmission electron micrographs of different CM-x samples at different resolutions. The surface of the material displays dense, wrinkled, and chaotically layered nanodomains, which are the result of the disordered, chaotic structure of the hard carbon material after high-temperature carbonization. This is consistent with the short-range disorder characteristic of hard carbon materials, indicating successful preparation. A graphite-like structure can be observed as the carbonization temperature increases.
[0057] XPS can also be used to analyze surface chemistry and functional group evolution. Figure 6The XPS spectra of the samples at three carbonization temperatures are shown. It can be seen from the figure that the two peaks at 532.5eV and 284.8eV correspond to the characteristic peaks of O1s and C1s, respectively, which are mainly composed of C and O elements. In order to further analyze the chemical state changes of carbon elements after sulfonation and high-temperature carbonization, the C1s peak is decomposed into four peaks, such as Figure 4 b. The surface of the carbon material contains oxygen atoms and the oxygen atoms mainly exist in the form of C=O bonds (located at 292eV in the C1s diagram), CO bonds (located at 287eV in the C1s diagram), CS bonds (located at 285.5eV in the C1s diagram) and CC / C=C bonds (located at 284.8eV in the C1s diagram). The oxygen-containing functional groups on the surface of the sample mainly come from the sulfonation process. These oxygen-containing functional groups can effectively increase the Na + The S2p characteristic peak of the CM-1300 sample is more obvious, which may be due to the insufficient carbonization temperature of CM-1200 and the excessively high carbonization temperature of CM-1400, resulting in excessive loss of oxygen atoms.
[0058] Example 2
[0059] Electrochemical performance
[0060] Sodium battery preparation:
[0061] To compare the effects of hard carbons prepared at different temperatures on the performance of sodium-ion batteries, button cells were assembled in an argon-filled, dual-station glove box. The hard carbons prepared at three carbonization temperatures, designated CM-1200, CM-1300, and CM-1400, were mixed in a ball mill at a ratio of 8:1:1 (CM-x:CMC:conductive carbon black). An appropriate amount of deionized water was added, and the mill was then placed in a carbon black fine grinder and stirred at 400 rpm for 3-4 hours to obtain a slurry of appropriate viscosity. This slurry was then evenly applied to a clean copper foil cleaned with anhydrous ethanol using a spatula on a dry cast coater and dried at 80°C for 20 minutes. After vacuum drying for 8 hours, the resulting electrode sheets were punched into circular electrodes with a diameter of 12 mm using a button cell slicer. The electrode sheets were weighed on an electronic analytical balance and the mass of the blank copper foil was subtracted from the mass of the two to obtain the mass of active material contained in the electrode sheets. Coin cells were assembled in a glove box using weighed electrode sheets, button cell casings, button cell springs, button cell spacers, glass fiber, commercial button cell sodium sheets, and NaPF6 electrolyte. Electrochemical constant-current charge-discharge tests were performed at room temperature using a Xinwei battery system.
[0062] Electrochemical analysis:
[0063] Figure 7 ac is a scan rate of 0.0001V s -1The cyclic voltammetry curve of the CM-x electrode shows that during the initial cycle, the irreversible reduction peak around 0.2-1.5V is caused by the irreversible decomposition of the electrolyte and the formation of the SEI film. Among them, the irreversible process of CM-1300 is the smallest during the initial cycle. On the CV curve, a sharp peak appears near 0.1-0.2V and a weak peak appears near 0.2-1.5V, corresponding to Na + interlayer insertion mechanism and surface adsorption process.
[0064] The constant current charge and discharge curve (1C = 300mA g) was tested at 0.1C (25℃) -1 ) to evaluate the electrochemical Na + Storage behavior, such as Figure 7 df. It's worth noting that all charge-discharge curves consist of two regions: a plateau capacity region below 0.1V and a slope capacity region above 0.1V, corresponding to the sharp peak in the low-voltage region and the low peak in the high-voltage region of the CV curve, respectively. CM-1200 exhibits a lower plateau capacity because the interlayer spacing is too wide, hindering Na+ adsorption.
[0065] The results showed that the reversible Na + Storage capacity is 196.89mAh g -1 , which is not satisfactory, with an ICE value of 76.5%. As the carbonization temperature increases, the microstructure of CM-x becomes disordered and the interlayer spacing expands, so the reversible Na + Storage capacity increased from 196.89mAh g in CM-1200 -1 Gradually increased to 264.03mAh g for CM-1300 -1 CM-1300 has the best interlayer spacing and achieved 264.03 mAh g -1 However, too high a carbonization temperature will reduce the interlayer spacing and affect the Na + insertion adsorption, thereby making Na + Storage performance is reduced. Therefore, the Na + The storage capacity has dropped to 211.90mAh g -1 . Figure 7 g A detailed comparison of the second CV curves between CM-x shows that CM-1300 has the largest CV area, further indicating that CM-1300 has the best storage capacity. Figure 7 h and Figure 7 The variation of platform capacity with carbonization temperature is summarized. Due to the higher carbonization temperature, there are more graphite-like structure phases, and the interlayer spacing (0.36-0.40 nm) is suitable for Na +The adsorption and release of the platform capacity gradually increased, and the platform capacity ratio increased from 59.92% of CM-1200 to 65.35% of CM-1300. However, the platform capacity ratio of CM-1400 was 62.83%, which may be due to excessive carbonization, which leads to a reduction in defects and further reduction in interlayer spacing. + The adsorption of the ions is affected, resulting in a decrease in the platform capacity.
[0066] Figure 8 The cyclic stability test of CM-x at currents of 0.1C, 0.5C, and 1C, and potential range of 0.001-3.0V, respectively. CM-x carbonized at higher temperatures showed a more disordered microstructure, which facilitated the Na + Adsorption and release process. At the same time, the rich oxygen-containing groups are Na + The storage of carbonized carbon provides reversible adsorption sites, which is also conducive to the improvement of cycling stability because little structural change occurs during the adsorption and release process. The results show that with the increase of carbonization temperature, the capacity retention rates of CM-1200, CM-1300 and CM-1400 after 50 cycles at 0.1C are 84.74%, 85.63% and 89.60%, respectively. The capacity retention rates of 0.5C and 1C after 100 cycles gradually increased from 73.42% of CM-1200 to 74.61% of CM-140 and from 64.86% of CM-1200 to 77.98%, respectively. Among them, CM-1300 maintained 277.77, 232.77 and 178.91 mAh g at different current densities, respectively. -1 The high storage capacity, capacity retention rate is 85.63%, 70.30%, and 66.40% respectively. From the data, it can be seen that CM-1400 has the highest capacity retention rate at different current densities. This may be because it produces more graphite-like structures after high-temperature carbonization, which makes it have a higher capacity retention rate, demonstrating its competitiveness as a practical negative electrode. Figure 8 As shown in Figure d, CM-1300 also has good rate performance. Its maximum reversible capacity is 259.2, 198.8, 103.0, and 75.66 mAh g at 0.1, 0.2, 0.5, and 1 C, respectively. -1 Since the rate performance depends on the electronic and ionic conductivity of the electrode, CM-1300 and CM-1400, based on their graphite-like structure and superior electronic conductivity, showed better rate performance at a high current of 2C, with retention capacities of 52.38 and 50.73 mAh g, respectively. -1 Furthermore, when the current rate was restored to 0.1C, the capacity of each sample could be recovered to the initial level, indicating that the robust structure of CM-x can withstand repeated charge and discharge processes at high rates.
[0067] Figure 8 e depicts the electrochemical impedance spectroscopy (EIS) of the CM-x electrode, with the inset showing the corresponding equivalent circuit. The Nyquist plot consists of a semicircle at mid-frequency and a sloped line at low frequency, corresponding to the charge transfer resistance (Rct) and Warburg impedance (W), respectively. In CM-x, the charge transfer resistance (Rct) increases from 98.5Ω to 225.5Ω when the carbonization temperature increases from 1200°C to 1400°C, likely due to the increase in oxygen-containing functional groups, which are detrimental to the charge transfer process. Furthermore, the slope of the line in the low-frequency region for the CM-1300 electrode becomes steeper, indicating that the enhanced structural disorder facilitates ion diffusion, while the high carbonization temperature for CM-1400 may reduce the interlayer spacing, thereby affecting ion diffusion.
[0068] In order to verify the practical application prospects of the prepared PP hard carbon anode, a full battery was assembled with CM-1300 as the anode and Na2Ti3O7 as the cathode. Figure 8 According to the mass of the active material of the negative electrode, the capacity at 0.1C is 218.07 mAh g -1 ( Figure 8 g). The long-term cycling performance of the full cell at 0.1C is shown, achieving a capacity retention of 98.90% after 100 cycles, demonstrating the practical application potential of PP materials.
[0069] The above disclosure is only a preferred embodiment of the method for preparing hard carbon and sodium ion batteries for masks of the present invention and its application. Of course, this cannot be used to limit the scope of the rights of the present invention. Ordinary technicians in this field can understand that implementing all or part of the processes of the above embodiments and making equivalent changes in accordance with the claims of the present invention still fall within the scope of the invention.
Claims
1. A method for preparing hard carbon for a mask, characterized in that: The following steps are involved: Cut the mask into small pieces and immerse them in concentrated sulfuric acid, then sulfonate them in an oil bath at a constant temperature to obtain a sulfide material; The sulfide material is diluted with clean water until the pH reaches neutral, and then dried to obtain black sulfide; Pre-carbonizing the black sulfide in a tube furnace in an argon environment by heating the black sulfide in stages to obtain a pre-carbonized product; The pre-carbonized products were divided into three groups and carbonized at different temperatures in a vertical high-temperature experimental furnace in an argon atmosphere to obtain hard carbon.
2. A method for preparing hard carbon for a mask as claimed in claim 1, characterized in that: The constant temperature sulfonation conditions are as follows: an oil bath at 180° C., stirring at a rate of 600 rpm, and a constant temperature sulfonation time of 3 hours.
3. A method for preparing hard carbon for a mask as claimed in claim 1, characterized in that: The specific method of diluting the sulfide material with clean water until the pH reaches neutral, and then drying it to obtain the black sulfide is as follows: Diluting the sulfide material with clean water, extracting the supernatant after precipitation, and leaving the precipitate; Repeatedly diluting the precipitate with clean water and testing the pH until the pH of the precipitate reaches neutral to obtain a central precipitate; The central precipitate was dried at 100° C. for 10 hours using a constant temperature air blower dryer to obtain a black sulfide.
4. A method for preparing hard carbon for a mask as claimed in claim 1, characterized in that: The staged heating pre-carbonization is divided into three stages. In the first stage, the temperature is increased to 300°C at a heating rate of 2°C / min and kept warm for 2 hours. In the second stage, the temperature is increased to 500°C at a heating rate of 2°C / min and kept warm for 2 hours. In the third stage, the temperature is increased to 900°C at a heating rate of 2°C / min and kept warm for 2 hours.
5. An application of hard carbon in preparing sodium ion batteries, applied to a method for preparing hard carbon for a mask as claimed in any one of claims 1 to 4, The method includes using the prepared hard carbon to prepare an electrode sheet, assembling the electrode sheet, a button battery shell, a button battery shrapnel, a button battery gasket, glass fiber, a commercial button battery sodium sheet and a NaPF6 electrolyte into a button battery in a glove box, and conducting an electrochemical constant current charge and discharge test at room temperature using a Xinwei battery system.
Citation Information
Patent Citations
Method for preparing negative electrode material of sodium ion battery from waste medical masks
CN113716547A
Mask-based sulfur-rich porous carbon material as well as preparation method and application thereof
CN115910619A
Lignin-phenolic resin-based hard carbon material as well as preparation method and application thereof
CN117326546A