Biomass-based hard carbon material, preparation method thereof and sodium ion battery
By controlling the hydrogen peroxide treatment conditions and carbonization temperature, biomass-based hard carbon materials with specific microstructures were prepared, which solved the problem of low performance of biomass-based hard carbon materials, improved the capacity and efficiency of sodium ion batteries, and achieved Stable cycle performance.
Patent Information
- Application Number
- CN202411402353.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-10-09
AI Technical Summary
The capacity of biomass-based hard carbon materials in sodium ion batteries and the efficiency of first-time Coulombs is low, and the complex composition affects the carbon structure and performance, which is unclear, making it difficult to control.
Lignocellulose-containing as the precursor, 2%-10% hydrogen peroxide solution was used to treat it at 25-80°C, and the solution pH was controlled to be 3-9. After washing and drying, carbonization was carried out under an inert atmosphere to prepare irregularities. Blocky biomass-based hard carbon material has short-range order and long-range disordered microstructure characteristics, controlling the pore structure and oxidation degree to improve performance.
The rapid diffusion of sodium ions is achieved, the rate performance of hard carbon, the battery capacity and first-time Coulomb efficiency are improved, and the circulation performance is stable.
Smart Images

Figure CN118978148A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of new energy materials, and in particular relates to a biomass-based hard carbon material and a preparation method thereof, and a sodium ion battery. Background Art
[0002] As an element of the same main group, sodium has similar physical and chemical properties to lithium, and sodium sources are abundant and inexpensive. Therefore, in recent years, sodium-ion batteries are considered to be the best supplement to lithium-ion batteries in the field of large-scale energy storage. Hard carbon is equivalent to graphite in lithium-ion batteries in the negative electrode material of sodium-ion batteries, but currently the hard carbon materials with excellent performance are mainly resin-based hard carbon, and its high cost limits its commercialization; while biomass-based hard carbon has broad commercial application prospects due to its wide source of raw materials and low price.
[0003] At present, biomass-based hard carbon materials still have the disadvantages of low capacity and first coulombic efficiency. Due to the complex composition of biomass and the unclear influence of each component on the carbon structure and performance, how to accurately modify the composition of biomass to control the final carbon pore structure and carbon layer spacing and improve the sodium storage performance of hard carbon has become a focus issue. Summary of the invention
[0004] In view of this, an embodiment of the present application provides a biomass-based hard carbon material, aiming to solve the problems of low capacity and first coulombic efficiency of existing biomass-based hard carbon materials.
[0005] The first aspect of the embodiment of the present application provides a biomass-based hard carbon material, wherein the morphology of the biomass-based hard carbon material is irregular block-shaped and there is a microporous structure on the surface; wherein the size of the irregular block is 5-10 μm; and the pore diameter of the microporous structure is less than 1 μm;
[0006] The biomass-based hard carbon material has microstructural characteristics of short-range order and long-range disorder.
[0007] In a possible implementation of the first aspect, the biomass-based hard carbon material is prepared by using lignocellulose-containing biomass as a precursor, treating it with a 2%-10% hydrogen peroxide solution at a temperature of 25-80°C for 1-6 hours, and controlling the pH value of the solution to be 3-9. After washing and drying, the material is carbonized under an inert atmosphere.
[0008] A second aspect of the embodiment of the present application provides a method for preparing the biomass-based hard carbon material described in the first aspect, comprising:
[0009] Treating the pretreated lignocellulose-containing biomass with a 2%-10% hydrogen peroxide solution at 25-80° C. for 1-6 hours, and controlling the pH of the solution to be 3-9, to obtain a reaction solution;
[0010] After the reaction solution is filtered, the obtained powder is washed to neutrality and dried;
[0011] The dried powder is carbonized under the protection of an inert atmosphere to obtain a biomass-based hard carbon negative electrode material.
[0012] A third aspect of an embodiment of the present application provides an electrode material, characterized in that the electrode material comprises a conductive additive, a binder and the biomass-based hard carbon material described in the first aspect.
[0013] A fourth aspect of an embodiment of the present application provides a negative electrode plate for a sodium ion battery, the negative electrode plate comprising a current collector, a conductive additive coated on the current collector, a binder, and the biomass-based hard carbon material described in the first aspect above.
[0014] A fifth aspect of an embodiment of the present application provides a sodium ion battery, comprising the negative electrode plate described in the fourth aspect.
[0015] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:
[0016] The embodiments of the present application provide a biomass-based hard carbon material having short-range order and long-range disorder microstructural characteristics, and its morphology is irregular block-shaped and there is a microporous structure on the surface. The size of the irregular block is 5-10 μm, and the pore diameter of the microporous structure is less than 1 μm, which is much smaller than the pore diameter of the existing hard carbon materials. Compared with the existing hard carbon materials, the biomass-based hard carbon material can achieve rapid diffusion of sodium ions, which is beneficial to improving the rate performance of hard carbon.
[0017] Furthermore, the present application embodiment also provides one of the preparation methods of the above-mentioned biomass-based hard carbon material, which uses a wide range of lignocellulose-containing biomass as raw materials, and has a simple preparation process and low cost. On the one hand, by changing the pH, the selective oxidation of lignin and cellulose by hydrogen peroxide can be controlled, thereby controlling the pore structure of the hard carbon and directionally improving the platform capacity and slope capacity of the hard carbon; on the other hand, by changing the reaction temperature, reaction time and hydrogen peroxide concentration, the degree of oxidation can be controlled, thereby achieving the purpose of controlling the specific surface area of the hard carbon and improving the first coulombic efficiency.
[0018] In addition, the sodium ion battery using the biomass-based hard carbon material provided in the embodiments of the present application has a high capacity and first coulombic efficiency and stable cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a SEM image of the biomass-based hard carbon material provided in Example 2 of the present application;
[0020] Figure 2The XRD pattern of the biomass-based hard carbon material provided in Example 2 of the present application;
[0021] Figure 3 This is a SEM image of the biomass-based hard carbon material provided in Example 4 of the present application;
[0022] Figure 4 The XRD pattern of the biomass-based hard carbon material provided in Example 4 of the present application;
[0023] Figure 5 This is a SEM image of the biomass-based hard carbon material provided in Example 6 of the present application;
[0024] Figure 6 The XRD pattern of the biomass-based hard carbon material provided in Example 6 of the present application;
[0025] Figure 7 This is a SEM image of the biomass-based hard carbon material provided in Comparative Example 1 of the present application;
[0026] Figure 8 This is the XRD diagram of the biomass-based hard carbon material provided in Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0028] An embodiment of the present application provides a biomass-based hard carbon material, which has an irregular block shape and a microporous structure on the surface; wherein the size of the irregular block is 5-10 μm; the pore diameter of the microporous structure is less than 1 μm; and the biomass-based hard carbon material has short-range order and long-range disorder microstructure characteristics.
[0029] Optionally, the biomass-based hard carbon material is prepared by using lignocellulose-containing biomass as a precursor, treating it with a 2%-10% hydrogen peroxide solution at 25-80° C. for 1-6 hours, controlling the pH of the solution to be 3-9, and then washing and drying it, and then carbonizing it under inert atmosphere protection;
[0030] Optionally, the material selection requirements for biomass containing lignocellulose in the present application are limited to biomass materials containing lignin and cellulose, such as one or more selected from bamboo, cork, coconut shell, walnut shell, poplar, apricot shell, lignin, cellulose, and tea oil shell; the selected biomass material is then peeled and mechanically crushed, such as bamboo powder can be obtained by drying and peeling 2-3 year old bamboo stems, and then mechanically crushing and passing through a 50-mesh sieve. Although the present application only uses bamboo as an example in the specific embodiments, this should not limit the scope of protection of the present application. Those skilled in the art can also replace bamboo with one or more of other cork, coconut shell, walnut shell, poplar, apricot shell, lignin, cellulose, and tea oil shell to achieve the same effect.
[0031] The present application also provides a method for preparing a biomass-based hard carbon material with a simple preparation process, low cost, adjustable platform capacity, high sodium storage capacity, and high energy density, comprising the following steps:
[0032] Step S1: treating the pretreated lignocellulose-containing biomass with a 2%-10% hydrogen peroxide solution at 25-80° C. for 1-6 hours, and controlling the pH of the solution to be 3-9 to obtain a reaction solution.
[0033] In the embodiments of the present application, pretreatment of the lignocellulose-containing biomass refers to removing impurities and sterilizing the biomass. As an example, the pretreatment method may be to crush the biomass into powder, sieve through a 50-mesh sieve, and then boil it in deionized water for 30 minutes.
[0034] In the embodiments of the present application, the pH condition can be controlled by adding an acid or a base to the system solution. For example, the acid for controlling the pH can be selected from one or more of hydrochloric acid, sulfuric acid, acetic acid, citric acid, phosphoric acid, and nitric acid; the base for controlling the pH can be selected from one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, sodium bicarbonate, and potassium bicarbonate. It is worth noting that the control of pH conditions is particularly critical. By changing the pH, the selective oxidation of lignin and cellulose by hydrogen peroxide can be controlled, thereby controlling the pore structure of hard carbon and directionally increasing the platform capacity and slope capacity of hard carbon. Therefore, the pH is preferably controlled to 3-7, more preferably 3.
[0035] In the embodiments of the present application, the control of reaction temperature, reaction time and hydrogen peroxide concentration is also particularly critical. By changing the reaction temperature, reaction time and hydrogen peroxide concentration, the degree of oxidation can be controlled, thereby achieving the purpose of controlling the hard carbon specific surface area and improving the first coulombic efficiency. Therefore, the reaction temperature is preferably controlled to 60-70°C. Since the temperature may fluctuate within the range of ±5°C during the reaction, it is preferably controlled to 65±5°C; the reaction time is preferably controlled to 1-3h, more preferably 3h; the concentration of the hydrogen peroxide solution is preferably controlled to 2%-6%, more preferably 6%.
[0036] Step S2: After the reaction solution is filtered, the obtained powder is washed to neutrality and dried.
[0037] Optionally, the reaction solution is filtered, the powder is washed with deionized water until it is neutral, and then placed in an oven at 105° C. to dry to a constant weight.
[0038] Step S3: The dried powder is carbonized under an inert atmosphere to obtain a biomass-based hard carbon negative electrode material.
[0039] Optionally, the dried powder is placed in a tubular furnace, protected by inert gas, and treated at 1100-1500°C for 1-3 hours to carbonize the material. After cooling to room temperature, the obtained carbon powder is crushed at high speed to obtain a biomass-based hard carbon material with irregular block-like macroscopic morphology and a pore structure on the surface. The typical size of the irregular blocks is 5-10μm, and the pore diameter of the pore structure is less than 1μm. The biomass-based hard carbon material has the microstructural characteristics of short-range order and long-range disorder.
[0040] Optionally, the inert gas may be one or more of argon and nitrogen.
[0041] Optionally, the heating rate is 2 to 10° C. / min.
[0042] Among them, the above-mentioned carbonization temperature, time and heating rate can all be set with reference to the existing technology. Although the following specific embodiments only use a single parameter as an example, it should not be used to limit the scope of protection of the present application. Those skilled in the art can adjust the settings of the carbonization temperature, time and heating rate according to the existing technology.
[0043] The biomass-based hard carbon material provided in the embodiments of the present application can be used to prepare electrode materials. Specifically, the electrode material includes a conductive additive, a binder and the above-mentioned biomass-based hard carbon material.
[0044] The biomass-based hard carbon material provided in the embodiment of the present application can be used to prepare the negative electrode plate of the sodium ion battery, and further used in the sodium ion secondary battery; specifically, the negative electrode plate includes a current collector, a conductive additive coated on the current collector, a binder and the above-mentioned biomass-based hard carbon material.
[0045] Among them, the types of the above-mentioned conductive additives, binders, and current collectors can be selected by referring to the existing technology. As an example, the conductive additive can be a carbon material, including one or more of carbon black, acetylene black, carbon fiber, conductive graphite, carbon nanotubes, and graphene; the binder can be one or more of polyvinylidene fluoride, sodium alginate, sodium polyacrylate, and sodium carboxymethyl cellulose; the current collector can be one of copper foil and aluminum foil.
[0046] The biomass-based hard carbon material is described in detail with specific examples as follows. The experimental methods used in the following examples are conventional methods unless otherwise specified; the materials and reagents used are all commercially available unless otherwise specified.
[0047] Example 1
[0048] In this embodiment, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0049] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0050] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0051] Step S130, treating the bamboo powder with a 2% hydrogen peroxide solution at 65±5°C for 3h, and controlling the pH of the reaction to 3 with a 30% acetic acid solution;
[0052] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0053] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0054] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0055] Example 2
[0056] In this embodiment, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0057] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0058] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0059] Step S130, treating the bamboo powder with a 6% hydrogen peroxide solution at 65±5° C. for 3 h, and controlling the pH of the reaction to be 3 with a 30% acetic acid solution;
[0060] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0061] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0062] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0063] Example 3
[0064] In this embodiment, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0065] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0066] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0067] Step S130, treating the bamboo powder with a 10% hydrogen peroxide solution at 65±5° C. for 3 h, and controlling the pH of the reaction to 3 with a 30% acetic acid solution;
[0068] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0069] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0070] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0071] Example 4
[0072] In this embodiment, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0073] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0074] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0075] Step S130, treating the bamboo powder with a 6% hydrogen peroxide solution at 65±5° C. for 3 h, and controlling the pH of the reaction to 7 with a 1 mol / L sodium hydroxide solution;
[0076] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0077] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0078] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0079] Example 5
[0080] In this embodiment, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0081] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0082] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0083] Step S130, treating the bamboo powder with a 6% hydrogen peroxide solution at 65±5° C. for 3 h, and controlling the pH of the reaction to 9 with a 1 mol / L sodium hydroxide solution;
[0084] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0085] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0086] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0087] Example 6
[0088] In this embodiment, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0089] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0090] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0091] Step S130, treating the bamboo powder with a 6% hydrogen peroxide solution at 25±5° C. for 3 h, and controlling the pH of the reaction to be 3 with a 30% acetic acid solution;
[0092] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0093] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0094] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0095] Example 7
[0096] In this embodiment, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0097] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0098] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0099] Step S130, treating the bamboo powder with a 6% hydrogen peroxide solution at 65±5° C. for 1 h, and controlling the pH of the reaction to be 3 with a 30% acetic acid solution;
[0100] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0101] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0102] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0103] Example 8
[0104] In this embodiment, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0105] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0106] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0107] Step S130, treating the bamboo powder with a 6% hydrogen peroxide solution at 65±5° C. for 6 hours, and controlling the pH of the reaction to 3 with a 30% acetic acid solution;
[0108] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0109] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0110] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0111] Comparative Example 1
[0112] In this comparative example, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0113] The bamboo powder was boiled for 30 minutes and dried in an oven at 105°C to constant weight; the bamboo powder was placed in a tubular furnace, and under argon protection, the temperature was raised to 1300°C at a rate of 2°C / min and kept warm for 3 hours to cause cracking and carbonization; the tubular furnace was naturally cooled to room temperature and then taken out.
[0114] Comparative Example 2
[0115] In this comparative example, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0116] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0117] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0118] Step S130, treating the bamboo powder with a 6% hydrogen peroxide solution at 65±5° C. for 3 h, and controlling the pH of the reaction to 12 with a 1 mol / L sodium hydroxide solution;
[0119] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0120] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0121] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0122] Comparative Example 3
[0123] In this comparative example, the method for preparing the biomass-based hard carbon material comprises the following steps:
[0124] Step S110, peeling the bamboo nodes, crushing them into powder by mechanical means, and passing through a 50-mesh sieve.
[0125] Step S120, transferring the bamboo powder into a beaker and boiling it with deionized water for 30 minutes.
[0126] Step S130, treating the bamboo powder with a 30% hydrogen peroxide solution at 65±5° C. for 3 h, and controlling the pH of the reaction to 3 with a 30% acetic acid solution;
[0127] Step S140, filtering the reaction solution in step S130, washing the bamboo powder with deionized water until it is neutral, and drying it in an oven at 105°C to a constant weight.
[0128] Step S150, putting bamboo powder into a tube furnace, passing inert gas protection, and heat treating at 1300° C. for 3 hours at a heating rate of 2° C. / min to carbonize it;
[0129] Step S160, cooling to room temperature, and crushing at high speed to obtain a biomass-based hard carbon material with an irregular block-like macroscopic morphology and a microporous structure on the surface.
[0130] The microstructure and typical size of the biomass-based hard carbon materials prepared in the above-mentioned embodiments and comparative examples were observed by scanning electron microscopy (SEM), the carbon interlayer spacing of the hard carbon was measured by X-ray diffractometer (XRD), the average pore diameter of the hard carbon was measured by small angle X-ray scattering (SAXS), and the specific surface area of the hard carbon was obtained based on the BET theory by N2 desorption test. The test results are shown in Table 1.
[0131] in, Figure 1-2 They are respectively the SEM image and XRD image of the biomass-based hard carbon material prepared in Example 2 above; Figure 3-4 They are respectively the SEM image and XRD image of the biomass-based hard carbon material prepared in the above Example 4; Figure 5-6 They are respectively the SEM image and XRD image of the biomass-based hard carbon material prepared in the above Example 6; Figure 7-8 They are respectively the SEM image and XRD image of the biomass-based hard carbon material prepared in the above comparative example 1.
[0132] Table 1
[0133]
[0134]
[0135] Furthermore, the biomass-based hard carbon material prepared in each embodiment is applied to the negative electrode of the sodium ion battery as the negative electrode active material of the sodium ion secondary battery. According to the mass ratio of 92%:3%:1.5%:3.5%, 184 mg of the above hard carbon powder, 6 mg of conductive carbon black, 6 mg of 2% (w / w) carboxymethyl cellulose solution, and 17.5 mg of 40% (w / w) styrene-butadiene rubber are weighed, and an appropriate amount of deionized water is added, and stirred for 20 minutes until it becomes a uniform slurry. A 100 μm scraper is used to evenly coat it on the surface of the copper (Cu) foil, and it is dried in a blast drying oven at 105°C for 2 hours. The Cu foil with active materials is cut into disc-shaped negative electrode sheets, and then transferred to the glove box for standby use.
[0136] The assembly of the simulated battery was carried out in a MIKROUNA glove box filled with Ar atmosphere, using the prepared carbon material pole piece as the negative electrode, the commercial electrolyte 1.0 mol / L NaPF6 in DME as the electrolyte, and the Na metal sheet as the counter electrode to assemble the 2016 button cell. After the above battery was left for 12 hours, the first charge and discharge test was carried out at a rate of 0.1C, with a voltage range of 0 to 2V. A long cycle test was carried out at a rate of 1C. The electrochemical performance test results are shown in Table 2.
[0137] Table 2
[0138]
[0139]
[0140] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
[0141] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A biomass-based hard carbon material, It is characterized in that The biomass-based hard carbon material has an irregular block shape and a microporous structure on the surface; wherein the size of the irregular block is 5-10 μm; and the pore diameter of the microporous structure is less than 1 μm; The biomass-based hard carbon material has microstructural characteristics of short-range order and long-range disorder.
2. The biomass-based hard carbon material according to claim 1, It is characterized in that The biomass-based hard carbon material is prepared by using lignocellulose-containing biomass as a precursor, treating it with a 2%-10% hydrogen peroxide solution at a temperature of 25-80° C. for 1-6 hours, controlling the solution pH to be 3-9, washing, drying, and then carbonizing it under inert atmosphere protection.
3. The biomass-based hard carbon material according to claim 2, It is characterized in that The concentration of the hydrogen peroxide solution is 2%-6%; the temperature is 60-70°C; the time is 1-3h; and the pH is 3-7.
4. The biomass-based hard carbon material according to claim 2, It is characterized in that The concentration of the hydrogen peroxide solution is 6%; the temperature is 65±5°C; the time is 3h; and the pH is 3.
5. A method for preparing the biomass-based hard carbon material according to claim 1, It is characterized in that include: Treating the pretreated lignocellulose-containing biomass with a 2%-10% hydrogen peroxide solution at 25-80° C. for 1-6 hours, and controlling the pH of the solution to be 3-9, to obtain a reaction solution; After the reaction solution is filtered, the obtained powder is washed to neutrality and dried; The dried powder is carbonized under the protection of an inert atmosphere to obtain a biomass-based hard carbon negative electrode material.
6. The method for preparing the biomass-based hard carbon material according to claim 5, It is characterized in that The concentration of the hydrogen peroxide solution is 2%-6%; the temperature is 60-70°C; the time is 1-3h; and the pH is 3-7.
7. The method for preparing the biomass-based hard carbon negative electrode material according to claim 5, It is characterized in that The concentration of the hydrogen peroxide solution is 6%; the temperature is 65°C; the time is 3 hours; and the pH is 3.
8. An electrode material, It is characterized in that The electrode material comprises a conductive additive, a binder and the biomass-based hard carbon material according to any one of claims 1-4.
9. A negative electrode sheet for a sodium ion battery, It is characterized in that The negative electrode plate comprises a current collector, a conductive additive coated on the current collector, a binder and the biomass-based hard carbon material according to any one of claims 1-4.
10. A sodium ion battery, It is characterized in that The sodium ion battery comprises the negative electrode sheet according to claim 9.
Citation Information
Patent Citations
Biochar for enhancing soil self-repairing and preparation method and application thereof
CN111530413A
Preparation method of wood-based carbon nanotube composite conductive film
CN111647196A
Biomass hard carbon negative electrode material for sodium ion battery as well as preparation method and application of biomass hard carbon negative electrode material
CN113381016A
Hard carbon negative electrode material of sodium-ion battery based on shell biomass and preparation method of hard carbon negative electrode material
CN113666356A
Biomass-based carbon material as well as preparation method and application thereof
CN114455581A
Cited By
Phosphorus-doped biomass-based hard carbon material, negative electrode, sodium ion battery and preparation method
CN121063515A