Method for purifying impurity-containing manganese sulfate solution
Through two-stage extraction method and multi-stage extraction, washing and stripping treatment, the problem of battery-grade manganese sulfate in the prior art is difficult to remove calcium and copper impurities, and the efficient and low-cost preparation of battery-grade manganese sulfate solution is achieved, which improves the Manganese yield and product purity.
Patent Information
- Application Number
- CN202411049423.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
When the existing solvent extraction method prepares battery-grade high-purity manganese sulfate, it is difficult to effectively remove impurities such as calcium and copper, resulting in high manganese loss rate, complex process and high cost, which affects the quality of battery materials and the development of the new energy industry.
Using two-stage extraction method, first use P204 and LIX984N extraction agent for preliminary extraction, followed by deep extraction using P204 and TBP extraction agent for in-depth extraction, combined with saponification and stripping treatment, and the impurities such as calcium and copper were removed through multi-stage extraction and washing steps to increase manganese. yield and product purity.
It achieves efficient removal of impurities, reduces the manganese loss rate, simplifies the process flow, reduces production costs, and obtains high-quality battery-grade manganese sulfate solution, which is suitable for industrial production.
Smart Images

Figure CN118978183A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of battery material preparation, and in particular relates to a method for purifying a solution containing mixed manganese sulfate. Background Art
[0002] Battery-grade manganese sulfate (MnSO4·H2O) is a precursor for preparing lithium battery ternary cathode materials, and is also the basic raw material for preparing battery-grade high-purity manganese tetraoxide and high-purity manganese dioxide. It is widely used in the field of new energy batteries. The main difference between battery-grade manganese sulfate and industrial-grade manganese sulfate is that the metal ion requirements are different. Battery-grade manganese sulfate has extremely strict requirements on the content of various impurities, including copper, cadmium, iron, zinc and chromium. The content must be less than 1mg / L, the content of calcium, magnesium, sodium and silicon must be less than 5mg / L, and the lead content must be less than 3mg / L. In the process of producing battery-grade high-purity manganese sulfate, the removal of calcium and copper is very critical. They have an important impact on the quality of the material and will directly affect the operation of the battery.
[0003] At present, the methods for removing impurities from manganese sulfate solution include crystallization, chemical precipitation and solvent extraction, etc. Among them, solvent extraction is a commonly used purification method in the process of preparing battery-grade high-purity manganese sulfate.
[0004] Solvent extraction has the advantages of short process, high efficiency and low energy consumption, and is considered to be the most promising method for deep removal of impurities such as calcium and copper from manganese sulfate solution. However, the current solvent extraction method still has the following defects: when using conventional extractants to produce battery-grade manganese sulfate, due to the low separation coefficient between calcium, copper and manganese, it is difficult to effectively remove impurities such as calcium and copper while ensuring the yield of manganese, resulting in poor product quality and high manganese loss rate; the process is complex, the number of extraction stages is large, and the consumption of auxiliary materials is high, resulting in high costs; and there are many by-products, which need to be sent to the back-end process for treatment, which is costly and puts great pressure on environmental protection.
[0005] In the process of preparing battery-grade manganese sulfate using impurity-containing manganese sulfate solution, impurity removal is a major focus. If the impurity metal ions in the impurity-containing manganese sulfate solution can be removed as much as possible and the manganese yield can be controlled, not only high-quality battery-grade manganese sulfate can be prepared, but also the pressure on manganese metal resources can be reduced, and the stable development of the new energy industry can be promoted. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the related art. To this end, the present invention provides a purification method for a manganese sulfate solution containing impurities, through which a refined manganese sulfate solution with impurity requirements meeting battery-grade manganese sulfate can be obtained, and efficient impurity removal of the manganese sulfate solution containing impurities is achieved. The process has the advantages of short process flow, low production cost and simple process control.
[0007] The above technical objectives of the present invention are achieved through the following technical solutions:
[0008] A method for purifying a solution containing impure manganese sulfate comprises the following steps:
[0009] (1) mixing a first organic phase containing a P204 extractant and a LIX984N extractant with a saponifying agent for a first saponification, performing a first extraction on a manganese sulfate solution to obtain a first loaded organic phase, performing a first washing on the first loaded organic phase to remove manganese to obtain a first manganese-containing wash water, and mixing the first manganese-containing wash water with a raffinate obtained by the first extraction to obtain a first raffinate;
[0010] (2) After the second organic phase containing the P204 extractant and the TBP extractant is mixed with a saponifying agent for a second saponification, the first raffinate obtained in step (1) is subjected to a second extraction to obtain a second loaded organic phase, the second loaded organic phase is subjected to a second washing to obtain a second manganese-containing wash water, the second manganese-containing wash water is mixed with the raffinate obtained by the second extraction to obtain a second raffinate, and the second raffinate is the refined manganese sulfate solution.
[0011] In one embodiment, in step (1), the first organic phase is composed of P204 extractant, LIX984N extractant and kerosene in a volume ratio of (1-2):1:(7-8), wherein the P204 extractant refers to diisooctyl phosphate extractant, and the LIX984N extractant is obtained by mixing 5-nonyl oxime and 2-hydroxy-5-nonyl acetophenone oxime in a volume ratio of 1:1.
[0012] In one embodiment, in step (1), the first organic phase is composed of P204 extractant, LIX984N extractant and kerosene in a volume ratio of (1-1.6):1:(7-7.8).
[0013] In one embodiment, in step (1) and step (2), the saponifying agent is at least one of sodium hydroxide and ammonia water, and the concentration of the saponifying agent is 6-15 mol / L.
[0014] In one embodiment, in step (1) and step (2), the saponifying agent is at least one of sodium hydroxide and ammonia water, and the concentration of the saponifying agent is 8-12 mol / L.
[0015] In one embodiment, in step (1) and step (2), the first saponification and the second saponification are performed at levels 1-5, and the saponification rate is 20-40%.
[0016] In one embodiment, in step (1) and step (2), the first saponification and the second saponification are performed at levels 2-5, and the saponification rate is 25-35%.
[0017] In one embodiment, in step (1) and step (2), the stages of the first extraction and the second extraction are 3-10, and the O / A ratio between the first extraction and the second extraction is 1-4.
[0018] In one embodiment, in step (1) and step (2), the stages of the first extraction and the second extraction are 5-8 stages, and the relative O / A ratio between the first extraction and the second extraction is 1.5-3.
[0019] In one embodiment, in step (1) and step (2), the first washing and the second washing refer to washing the first loaded organic phase and the second loaded organic phase respectively with a sulfuric acid solution having a concentration of 0.1-2.5 mol / L.
[0020] In one embodiment, in step (1) and step (2), the first washing and the second washing refer to washing the first loaded organic phase and the second loaded organic phase respectively with a sulfuric acid solution having a concentration of 0.5-2 mol / L.
[0021] In one embodiment, in step (1) and step (2), the number of stages of the first washing and the second washing is 3-8.
[0022] In one embodiment, in step (1) and step (2), the number of stages of the first washing and the second washing is 4-7.
[0023] In one embodiment, in step (1), after the first loaded organic phase is subjected to the first washing to remove manganese, it is subjected to the first stripping to strip metal impurities therein, and then it is washed with water and then recycled to the first extraction stage as an extracted organic phase.
[0024] In one embodiment, the first stripping includes first stripping calcium and copper from the first loaded organic phase with a hydrochloric acid solution having a concentration of 4-5 mol / L, and then stripping iron, zinc, and aluminum from the first loaded organic phase with a hydrochloric acid solution having a concentration of 5.5-7 mol / L.
[0025] In one embodiment, in step (2), after the second loaded organic phase is subjected to the second washing to remove manganese, it is subjected to a second stripping to strip metal impurities therein, and then washed with water and recycled to the second extraction stage as an extracted organic phase.
[0026] In one embodiment, the second stripping includes first stripping calcium from the second loaded organic phase with a hydrochloric acid solution having a concentration of 4-5 mol / L, and then stripping iron, zinc, and aluminum from the second loaded organic phase with a hydrochloric acid solution having a concentration of 5.5-7 mol / L.
[0027] In one embodiment, in step (1) and step (2), the levels of the stripping extraction of calcium copper, the stripping extraction of calcium, and the stripping extraction of iron, zinc, and aluminum are all 4-9 levels.
[0028] In one embodiment, in step (1) and step (2), the levels of the stripping extraction of calcium copper, the stripping extraction of calcium, and the stripping extraction of iron, zinc, and aluminum are all 5-6 levels.
[0029] In one embodiment, in step (2), the second organic phase is composed of P204 extractant, TBP extractant and kerosene in a volume ratio of (1-3):1:(7-20), wherein the P204 extractant refers to diisooctyl phosphate extractant, and the TBP extractant refers to tributyl phosphate extractant.
[0030] In one embodiment, in step (2), the second organic phase is composed of P204 extractant, TBP extractant and kerosene in a volume ratio of (1.5-3):1:(7-18).
[0031] In one embodiment, in step (1) and step (2), the pH of the aqueous phase is controlled to be 1-3 during the first washing and the second washing.
[0032] In one embodiment, in step (1) and step (2), the pH of the aqueous phase is controlled to be 1.5-2.5 during the first washing and the second washing.
[0033] The beneficial effects of the present invention are:
[0034] (1) The present invention can obtain a refined manganese sulfate solution through a two-stage extraction method. The process has the characteristics of simple operation, high production efficiency, short process, high calcium, copper, zinc, iron and aluminum impurity removal rate, and easy control. Compared with other methods for purifying impure manganese sulfate solutions using solvent extraction, the present method can effectively remove calcium and copper impurities in the impurity manganese sulfate solution;
[0035] (2) The present invention first extracts and removes most of the Ca and Cu in the impurity-containing manganese sulfate solution by P204+LIX984N, wherein LIX984N is a copper extractant. The use of the copper extractant as a co-extractant for synergistic extraction greatly improves the copper-manganese separation coefficient, reduces the manganese loss rate while removing copper, and then deeply removes calcium from the raffinate removed by the P204+LIX984N process by P204+TBP, thereby achieving efficient removal of impurities such as calcium and copper;
[0036] (3) The method of the present invention overcomes the problems of the existing purification methods, that is, the purity of battery-grade manganese sulfate is not high enough and the impurity metal content is high, and a high-quality manganese sulfate solution is obtained. Moreover, the whole process is carried out under normal pressure, and temperature control is not required, which is conducive to industrial production.
[0037] (4) In the two-stage extraction process described in the present invention, the extraction and washing functional stages are set with fewer stages and smaller fluxes, so a smaller extraction tank can be used. Less extractant and stock solution are required in the tank filling work before extraction, and the cost investment is low. In addition, the present invention adopts an extraction method with low auxiliary material consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a schematic diagram of the process of Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The present invention will be further described below in conjunction with specific embodiments.
[0040] Embodiment 1:
[0041] A method for purifying a solution containing manganese sulfate, such as Figure 1 As shown: the following steps are included:
[0042] (1) P204 extractant, LIX984N extractant and kerosene were mixed in a volume ratio of 15:10:75 to prepare a first organic phase, and the first organic phase was subjected to a first saponification treatment using a 10 mol / L sodium hydroxide solution. The number of saponification stages was set to 2, and the saponification rate was controlled to be 30%. The first organic phase after saponification was subjected to a first extraction reaction with a manganese sulfate solution containing impurities at room temperature to extract impurity metals such as calcium, copper, zinc, iron, aluminum and part of manganese into the first organic phase to obtain a first loaded organic phase. The number of extraction stages was set to 8, and the flow rate of the pre-extraction liquid was 22 m 3 / h, each stage reaction time is 5 minutes, the relative O / A is controlled to 2, and then the first loaded organic phase enters the washing section and is washed with 2mol / L sulfuric acid solution. The washing stage is set to 6, and the washing acid flow rate is 0.8m 3 / h, each stage of reaction is 5 minutes, manganese is washed into the water phase to obtain manganese-containing washing water, the manganese-containing washing water is mixed with the raffinate obtained by the first extraction as the first raffinate, and then the washed first loaded organic phase enters the stripping section and first uses 4.5mol / L hydrochloric acid solution for stripping, calcium and copper are stripped into the water phase, the stripping stage number is set to 6, and then uses 6mol / L hydrochloric acid solution for stripping, iron, zinc and aluminum are stripped into the water phase, the stripping stage number is set to 6, and then the first loaded organic phase after stripping is washed with water until the hydrogen ion concentration in the washed liquid is less than 1.3mol / L, and then the washed organic phase is returned to the first extraction section, and the first raffinate enters the next step;
[0043] (2) P204 extractant, TBP extractant and kerosene were mixed in a volume ratio of 15:5:80 to prepare a second organic phase, and the second organic phase was subjected to a second saponification treatment using a 10 mol / L sodium hydroxide solution. The saponification stage number was set to 2, and the saponification rate was controlled to be 40%. The saponified second organic phase was subjected to a second extraction reaction with the first raffinate obtained in step (1) at room temperature to extract calcium and part of manganese into the second organic phase to obtain a second loaded organic phase. The extraction stage number was set to 5, and the pre-extraction liquid flow rate was 22 m 3 / h, each stage reaction time is 5 minutes, the relative O / A is controlled to 1.5, and then the second loaded organic phase enters the washing section and is washed with 0.5 mol / L sulfuric acid solution. The washing stage is set to 4, and the washing acid flow rate is 0.5m 3 / h, each stage of reaction lasts for 5 minutes, manganese is backwashed into the water phase to obtain manganese-containing washing water, the manganese-containing washing water is mixed with the raffinate obtained by the second extraction as the second raffinate, and then the second loaded organic phase enters the stripping section for stripping with a 4.5 mol / L hydrochloric acid solution, further stripping calcium into the water phase, the stripping section stage number is set to 5, and then stripping with a 6 mol / L hydrochloric acid solution, further stripping iron, zinc and aluminum into the water phase, the stripping section stage number is set to 5, and then the second loaded organic phase after stripping is washed with water until the hydrogen ion concentration in the washed liquid is less than 1.3 mol / L, and the washed organic phase is returned to the second extraction section, and the obtained second raffinate is the refined manganese sulfate solution.
[0044] Embodiment 2:
[0045] A method for purifying a solution containing impure manganese sulfate comprises the following steps:
[0046] (1) P204 extractant, LIX984N extractant and kerosene were mixed in a volume ratio of 15:10:75 to prepare a first organic phase, and the first organic phase was subjected to a first saponification treatment using a 10 mol / L sodium hydroxide solution. The number of saponification stages was set to 2, and the saponification rate was controlled to be 30%. The first organic phase after saponification was subjected to a first extraction reaction with a manganese sulfate solution containing impurities at room temperature to extract impurity metals such as calcium, copper, zinc, iron, aluminum and part of manganese into the first organic phase to obtain a first loaded organic phase. The number of extraction stages was set to 7, and the flow rate of the pre-extraction liquid was 21 m 3 / h, each stage reaction time is 6 minutes, the relative O / A is controlled to 2, and then the first loaded organic phase enters the washing section and is washed with 1.5 mol / L sulfuric acid solution. The washing stage is set to 5, and the washing acid flow rate is 1m 3 / h, each stage reaction time is 6 minutes, manganese is washed into the water phase to obtain manganese-containing washing water, the manganese-containing washing water is mixed with the raffinate obtained by the first extraction as the first raffinate, and then the washed first loaded organic phase enters the stripping section and first uses 4.5mol / L hydrochloric acid solution for stripping, calcium and copper are stripped into the water phase, the stripping section stage number is set to 6, and then uses 6mol / L hydrochloric acid solution for stripping, iron, zinc and aluminum are stripped into the water phase, the stripping section stage number is set to 6, and then the first loaded organic phase after stripping is washed with water until the hydrogen ion concentration in the washed liquid is less than 1.3mol / L, and then the washed organic phase is returned to the first extraction section, and the first raffinate enters the next step;
[0047] (2) P204 extractant, TBP extractant and kerosene were mixed in a volume ratio of 15:10:75 to prepare a second organic phase, and the second organic phase was subjected to a second saponification treatment using a 10 mol / L sodium hydroxide solution. The saponification stage number was set to 2, and the saponification rate was controlled to be 40%. The saponified second organic phase was subjected to a second extraction reaction with the first raffinate obtained in step (1) at room temperature to extract calcium and part of manganese into the second organic phase to obtain a second loaded organic phase. The extraction stage number was set to 5, and the pre-extraction liquid flow rate was 21 m 3 / h, the reaction time of each stage is 6 minutes, the relative O / A is controlled to 1.5, and then the second loaded organic phase enters the washing section and is washed with 1mol / L sulfuric acid solution. The washing stage is set to 4, and the washing acid flow rate is 0.8m 3 / h, the reaction time of each stage is 6 minutes, manganese is backwashed into the water phase to obtain manganese-containing washing water, the manganese-containing washing water is mixed with the raffinate obtained by the second extraction as the second raffinate, and then the second loaded organic phase enters the stripping section for stripping with a 4.5mol / L hydrochloric acid solution, further stripping calcium into the water phase, the stripping section stage number is set to 5, and then stripping with a 6mol / L hydrochloric acid solution, further stripping iron, zinc and aluminum into the water phase, the stripping section stage number is set to 5, and then the second loaded organic phase after stripping is washed with water until the hydrogen ion concentration in the washed liquid is less than 1.3mol / L, and the washed organic phase is returned to the second extraction section, and the obtained second raffinate is the refined manganese sulfate solution.
[0048] Embodiment 3:
[0049] A method for purifying a solution containing impure manganese sulfate comprises the following steps:
[0050] (1) P204 extractant, LIX984N extractant and kerosene were mixed in a volume ratio of 15:10:75 to prepare a first organic phase, and the first organic phase was subjected to a first saponification treatment using a 10 mol / L sodium hydroxide solution. The number of saponification stages was set to 2, and the saponification rate was controlled to be 30%. The first organic phase after saponification was subjected to a first extraction reaction with a manganese sulfate solution containing impurities at room temperature to extract impurity metals such as calcium, copper, zinc, iron, aluminum and part of manganese into the first organic phase to obtain a first loaded organic phase. The number of extraction stages was set to 7, and the flow rate of the pre-extraction liquid was 23 m 3 / h, each stage reaction time is 6 minutes, the relative O / A is controlled to 2, and then the first loaded organic phase enters the washing section and is washed with 1.5 mol / L sulfuric acid solution. The washing stage is set to 4, and the washing acid flow rate is 1.2m 3 / h, each stage reaction time is 6 minutes, manganese is washed into the water phase to obtain manganese-containing washing water, the manganese-containing washing water is mixed with the raffinate obtained by the first extraction as the first raffinate, and then the washed first loaded organic phase enters the stripping section and first uses 4.5mol / L hydrochloric acid for stripping, calcium and copper are stripped into the water phase, the stripping stage number is set to 6, and then uses 6mol / L hydrochloric acid for stripping, iron, zinc and aluminum are stripped into the water phase, the stripping stage number is set to 6, and then the first loaded organic phase after stripping is washed with water until the hydrogen ion concentration in the washed liquid is less than 1.3mol / L, and then the washed organic phase is returned to the first extraction section, and the first raffinate enters the next step;
[0051] (2) P204 extractant, TBP extractant and kerosene were mixed in a volume ratio of 15:5:80 to prepare a second organic phase, and the second organic phase was subjected to a second saponification treatment using a 10 mol / L sodium hydroxide solution. The saponification stage number was set to 2, and the saponification rate was controlled to be 40%. The saponified second organic phase was subjected to a second extraction reaction with the first raffinate obtained in step (1) at room temperature to extract calcium and part of manganese into the second organic phase to obtain a second loaded organic phase. The extraction stage number was set to 5, and the pre-extraction liquid flow rate was 22.5 m 3 / h, the reaction time of each stage is 6 minutes, the relative O / A is controlled to 1.5, and then the second loaded organic phase enters the washing section and is washed with 0.5mol / L sulfuric acid solution. The washing stage is set to 4, and the washing acid flow rate is 1.2m 3 / h, the reaction time of each stage is 6 minutes, manganese is backwashed into the water phase to obtain manganese-containing washing water, the manganese-containing washing water is mixed with the raffinate obtained by the second extraction as the second raffinate, and then the second loaded organic phase enters the stripping section for stripping with a 4.5mol / L hydrochloric acid solution, further stripping calcium into the water phase, the stripping section stage number is set to 5, and then stripping with a 6mol / L hydrochloric acid solution, further stripping iron, zinc and aluminum into the water phase, the stripping section stage number is set to 5, and then the second loaded organic phase after stripping is washed with water until the hydrogen ion concentration in the washed liquid is less than 1.3mol / L, and the washed organic phase is returned to the second extraction section, and the obtained second raffinate is the refined manganese sulfate solution.
[0052] Comparative Example 1: (The only difference from Example 1 is that the LIX984N extractant in step (1) of Example 1 is replaced by the M5640 extractant)
[0053] A method for purifying a solution containing impure manganese sulfate comprises the following steps:
[0054] (1) P204 extractant, M5640 extractant and kerosene were mixed in a volume ratio of 15:10:75 to prepare a first organic phase, and the first organic phase was subjected to a first saponification treatment using a 10 mol / L sodium hydroxide solution. The number of saponification stages was set to 2, and the saponification rate was controlled to be 30%. The first organic phase after saponification was subjected to a first extraction reaction with a manganese sulfate solution containing impurities at room temperature to extract impurity metals such as calcium, copper, zinc, iron, aluminum and part of manganese into the first organic phase to obtain a first loaded organic phase. The number of extraction stages was set to 8, and the flow rate of the liquid before extraction was 22 m 3 / h, each stage reaction time is 5 minutes, the relative O / A is controlled to 2, and then the first loaded organic phase enters the washing section and is washed with 2mol / L sulfuric acid solution. The washing stage is set to 6, and the washing acid flow rate is 0.8m 3 / h, each stage reaction time is 5 minutes, manganese is washed into the water phase to obtain manganese-containing washing water, the manganese-containing washing water is mixed with the raffinate obtained by the first extraction as the first raffinate, and then the washed first loaded organic phase enters the stripping section and first uses 4.5mol / L hydrochloric acid solution for stripping, calcium and copper are stripped into the water phase, the stripping section stage number is set to 6, and then uses 6mol / L hydrochloric acid solution for stripping, iron, zinc and aluminum are stripped into the water phase, the stripping section stage number is set to 6, and then the first loaded organic phase after stripping is washed with water until the hydrogen ion concentration in the washed liquid is less than 1.3mol / L, and then the washed organic phase is returned to the extraction section, and the first raffinate enters the next step;
[0055] (2) P204 extractant, TBP extractant and kerosene were mixed in a volume ratio of 15:5:80 to prepare a second organic phase, and the second organic phase was subjected to a second saponification treatment using a 10 mol / L sodium hydroxide solution. The saponification stage number was set to 2, and the saponification rate was controlled to be 40%. The saponified second organic phase was subjected to a second extraction reaction with the first raffinate obtained in step (1) at room temperature to extract calcium and part of manganese into the second organic phase to obtain a second loaded organic phase. The extraction stage number was set to 5, and the pre-extraction liquid flow rate was 22 m 3 / h, each stage reaction time is 5 minutes, the relative O / A is controlled to 1.5, and then the second loaded organic phase enters the washing section and is washed with 0.5 mol / L sulfuric acid solution. The washing stage is set to 4, and the washing acid flow rate is 0.5m 3 / h, the reaction time of each stage is 5 minutes, manganese is backwashed into the water phase to obtain manganese-containing washing water, the manganese-containing washing water is mixed with the raffinate obtained by the second extraction as the second raffinate, and then the second loaded organic phase enters the stripping section for stripping with a 4.5mol / L hydrochloric acid solution, further stripping calcium into the water phase, the stripping section stage number is set to 5, and then stripping with a 6mol / L hydrochloric acid solution, further stripping iron, zinc and aluminum into the water phase, the stripping section stage number is set to 5, and then the second loaded organic phase after stripping is washed with water until the hydrogen ion concentration in the washed liquid is less than 1.3mol / L, and the washed organic phase is returned to the second extraction section, and the obtained second raffinate is the refined manganese sulfate solution.
[0056] The extraction, washing and stripping operations involved in the above Examples 1-3 and Comparative Example 1 are all performed at room temperature if the temperature is not specifically specified, and are all performed at normal pressure if the pressure is not specifically specified.
[0057] Test example:
[0058] The concentrations of various metal elements in the manganese sulfate solution containing impurities used in Examples 1-3 of the present invention and Comparative Example 1 are shown in Table 1. The concentrations of metal elements in the refined manganese sulfate solutions obtained in Examples 1-3 and Comparative Example 1 are measured, and the results are shown in Table 2. The removal rate of impurity ions in the manganese sulfate solution containing impurities is calculated, and the results are shown in Table 3. The manganese yield is calculated, and the manganese yield is the ratio of the manganese content in the refined manganese sulfate solution produced per hour to the manganese content in the manganese sulfate solution containing impurities entering the system per hour. In Examples 1-3 and Comparative Example 1, the flow rate of the pre-extraction liquid in step (1) is measured as flow rate A, the flow rate of the pre-extraction liquid in step (2) is measured as flow rate B, the flow rate of the acid washing in step (2) is measured as flow rate C, the manganese concentration in the refined manganese sulfate solution is measured as concentration D, and the manganese concentration in the manganese sulfate solution containing impurities is measured as concentration E. The manganese yield = concentration D * (flow rate B + flow rate C) / (concentration E * flow rate A) * 100%. The calculated manganese yield is shown in Table 4.
[0059] Table 1: Concentration of metal elements in manganese sulfate solution (g / L)
[0060] Co2+ <![CDATA[Cu 2+ ]]> <![CDATA[Ni 2+ ]]> <![CDATA[Fe 3+ ]]> <![CDATA[Al 3+ ]]> <![CDATA[Mn 2+ ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Zn 2+ ]]> Example 1 0.005 0.924 0.008 0.015 0.022 91.216 0.817 0.009 0.011 Example 2 0.006 0.934 0.007 0.017 0.023 88.954 0.875 0.010 0.015 Example 3 0.005 0.953 0.009 0.019 0.025 93.458 0.956 0.007 0.017 Comparative Example 1 0.005 0.918 0.009 0.017 0.021 95.124 0.798 0.010 0.015
[0061] Table 2: Concentration of metal elements in refined manganese sulfate solution (g / L)
[0062] Co2+ <![CDATA[Cu 2+ ]]> <![CDATA[Ni 2+ ]]> <![CDATA[Fe 3+ ]]> <![CDATA[Al 3+ ]]> <![CDATA[Mn 2+ ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Zn 2+ ]]> Example 1 0.003 0.0018 0.005 0.00003 0.00016 89.173 0.0002 0.004 0.00004 Example 2 0.005 0.0007 0.004 0.00002 0.00016 85.642 0.0011 0.005 0.00007 Example 3 0.004 0.0016 0.007 0.00005 0.00021 90.156 0.0008 0.003 0.00009 Comparative Example 1 0.004 0.0173 0.006 0.00015 0.00016 90.157 0.0218 0.004 0.00052
[0063] Table 3: Impurity ion removal rate / %
[0064] <![CDATA[Ca 2+ ]]> <![CDATA[Cu 2+ ]]> <![CDATA[Zn 2+ ]]> <![CDATA[Fe 3+ ]]> <![CDATA[Al 3+ ]]> Example 1 99.98 99.81 99.64 99.80 99.27 Example 2 99.87 99.93 99.53 99.88 99.30 Example 3 99.92 99.83 99.47 99.74 99.16 Comparative Example 1 97.27 98.12 96.53 99.12 99.24
[0065] Table 4. Manganese yield
[0066]
[0067] As shown in Table 3, the purification method of the present invention has a significant effect on the Ca 2+ The removal rate of Cu 2+ The removal rate of Zn 2+ The removal rate of Fe 3+ The removal rate of Al 3+ The removal rate can reach 99.16%, and the removal rate of calcium, copper, zinc, iron and aluminum is high.
[0068] It can be seen from Table 4 that the manganese recovery rate of the purification method of the present invention can reach 99.40%, which can effectively reduce the loss rate of manganese.
[0069] By comparing Example 1 with Comparative Example 1, it can be seen that the impurity ion removal rate of the synergistic extraction of LIN984X extractant and P204 extractant is better than that of the synergistic extraction of M5640 copper extractant and P204 extractant. At the same time, by comparing Example 1 with Comparative Example 1, it can be seen that when the LIX984N extractant in step (1) is replaced by the M5640 extractant, the manganese yield obtained is reduced from 99.98% to 96.93%, indicating that the synergistic extraction of LIN984X extractant and P204 extractant can significantly improve the manganese yield.
Claims
1. A method for purifying a solution containing manganese sulfate, characterized in that: The following steps are involved: (1) mixing a first organic phase containing a P204 extractant and a LIX984N extractant with a saponifying agent for a first saponification, performing a first extraction on a manganese sulfate solution to obtain a first loaded organic phase, performing a first washing on the first loaded organic phase to remove manganese to obtain a first manganese-containing wash water, and mixing the first manganese-containing wash water with a raffinate obtained by the first extraction to obtain a first raffinate; (2) After the second organic phase containing the P204 extractant and the TBP extractant is mixed with a saponifying agent for a second saponification, the first raffinate obtained in step (1) is subjected to a second extraction to obtain a second loaded organic phase, the second loaded organic phase is subjected to a second washing to obtain a second manganese-containing wash water, the second manganese-containing wash water is mixed with the raffinate obtained by the second extraction to obtain a second raffinate, and the second raffinate is the refined manganese sulfate solution.
2. The method for purifying a solution containing manganese sulfate according to claim 1, characterized in that: In step (1), the first organic phase is composed of P204 extractant, LIX984N extractant and kerosene in a volume ratio of (1-2):1:(7-8).
3. The method for purifying a solution containing manganese sulfate according to claim 1, characterized in that: In step (1) and step (2), the saponifying agent is at least one of sodium hydroxide and ammonia water, and the concentration of the saponifying agent is 6-15 mol / L.
4. The method for purifying a solution containing manganese sulfate according to claim 1, characterized in that: In step (1) and step (2), the first saponification and the second saponification are set to levels 1-5, and the saponification rate is 20-40%.
5. The method for purifying a solution containing manganese sulfate according to claim 1, characterized in that: In step (1) and step (2), the stages of the first extraction and the second extraction are 3-10, and the O / A ratio of the first extraction and the second extraction is 1-4.
6. The method for purifying a solution containing manganese sulfate according to claim 1, characterized in that: In step (1) and step (2), the first washing and the second washing refer to washing the first loaded organic phase and the second loaded organic phase respectively with a sulfuric acid solution having a concentration of 0.1-2.5 mol / L.
7. The method for purifying a solution containing manganese sulfate according to claim 1, characterized in that: In step (1) and step (2), the number of stages of the first washing and the second washing is 3-8.
8. The method for purifying a solution containing manganese sulfate according to claim 1, characterized in that: In step (1), the first loaded organic phase is subjected to the first washing to remove manganese, and then subjected to the first stripping to strip metal impurities therein, and then is washed with water and recycled to the first extraction stage as an extracted organic phase.
9. The method for purifying a solution containing manganese sulfate according to claim 1, characterized in that: In step (2), the second loaded organic phase is subjected to the second washing to remove manganese, and then subjected to the second stripping to strip metal impurities therein, and then washed with water and reused in the second extraction stage as the extracted organic phase.
10. The method for purifying a solution containing manganese sulfate according to claim 1, characterized in that: In step (2), the second organic phase is composed of P204 extractant, TBP extractant and kerosene in a volume ratio of (1-3):1:(7-20).