Preparation method and application of cobalt lithium manganate
By using the ratio of excess cobalt to manganese and the hydrothermal-high temperature solid-phase method in lithium manganese, combined with ultrasonic treatment, the problem of poor circulation performance of lithium manganese battery is solved, and capacity improvement and safety improvement is achieved. Overall performance of lithium cobalt oxide batteries.
Patent Information
- Application Number
- CN202411184677.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-19
AI Technical Summary
Lithium manganate has fast capacity decay and is easily damaged during the circulation process. It is difficult for existing doping and surface treatment methods to improve capacity and circulation performance simultaneously.
The ratio of excess cobalt to manganese is adopted to prepare lithium cobalt manganese by hydrothermal-high temperature solid phase method and ultrasonic treatment to reduce particle agglomeration and improve the circulation performance and safety of battery materials.
It significantly improves the circulation performance and capacity of lithium manganese oxide batteries, is close to the performance of lithium cobalt oxide batteries, and improves the safety of the batteries, avoiding the risk of structural damage and overcharging and overdischarge.
Smart Images

Figure CN118978187A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy materials, and in particular to a preparation method of lithium cobalt manganese oxide and application thereof. Background Art
[0002] So far, most commercial lithium-ion battery positive electrode materials mainly use lithium cobalt oxide, but because cobalt resources are relatively scarce and expensive, the application of this material in large-scale power batteries is restricted. Among the many positive electrode materials for lithium-ion batteries, lithium manganese oxide is a material with relatively better application prospects. Due to the wide range of resources for synthetic lithium manganese oxide, lower prices, relatively more environmentally friendly, and potential excellent charge and discharge characteristics, it has become the focus of lithium-ion battery research and development in recent years. Spinel LiMn2O4 has a three-dimensional tunnel structure and can be charged and discharged quickly. In practical applications, the reversible capacity of the device reaches more than 120mAh / g, and the energy density reaches 70-80% of LiCoO2. However, its biggest disadvantage is that the capacity decays relatively quickly during the cycle. This is because there is a structural phase change during the charge and discharge process, and in the current electrolyte system, Mn occurs. 3+ The disproportionation reaction of lithium manganese oxide causes it to dissolve in the electrolyte, destroying the structure and surface properties of the material. In order to solve the problem of poor material cycle performance, people have conducted extensive research on this. Doping and surface treatment are two effective means to improve the cycle performance of materials. In previous studies, lithium was often used as the negative electrode for electrochemical performance testing. Since manganese dissolves during the charging and discharging process of lithium manganese oxide, and these dissolved manganese may be deposited on the surface of the negative electrode during the charging and discharging process, if a carbon negative electrode is used, its surface SEI film will be changed. Therefore, this factor must be considered in practical applications. In this study, the electrochemical properties of lithium manganese oxide were studied using an actual electrochemical system. However, in the process of preparing lithium cobalt manganese oxide precursor by hydrothermal method, particle agglomeration is prone to occur. During the high-temperature solid-phase sintering process, the particles will undergo secondary agglomeration, affecting the performance in the later stage.
[0003] In view of the above problems, although the performance of lithium manganese oxide has been improved to a certain extent by doping and surface treatment, the improvement of capacity and the cycle performance have not been well solved. Therefore, the present invention makes improvements in terms of safety, cycle performance and capacity improvement, so that the overall performance of the battery of the lithium manganese oxide system is better improved. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing lithium cobalt manganese oxide and its application in view of the above-mentioned problems, so as to achieve the goal of improving the cycle performance of lithium manganese oxide by doping through the ratio of excessive cobalt to manganese, and also to improve the capacity and cycle performance of the overall battery through excessive cobalt, while taking into account the safety of lithium manganese oxide, thereby achieving greater improvement in the overall performance of lithium manganese oxide batteries.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] The method for preparing lithium cobalt manganese oxide of the present invention comprises the following steps:
[0007] (1) The chemical formula of the lithium cobalt manganese oxide material is shown in formula (I),
[0008] LiCoxMn1-xO2; (I)
[0009] Among them, x>0, 1>1-x>0;
[0010] The lithium source, cobalt source and manganese source, additives and dispersants are mixed together to form a mixture, and the mixture is transferred into a planetary mill. Zirconia balls of different sizes are used. The mixture and the zirconium oxide balls are mixed at a weight ratio of 1:6 to 10. The mixture is taken out after 20-60 minutes of nodularity.
[0011] (2) The ground mixture is transferred into a hydrothermal reactor, the hydrothermal reactor is placed into an ultrasonic disperser, and then the ultrasonic disperser and the hydrothermal reactor are placed into a high-temperature oven. The heating rate of the oven is 1.5-3°C / min, and the maximum temperature of the oven is set to 180°C. After the temperature reaches the maximum temperature, it is kept warm for 10-20 hours. The ultrasonic disperser is turned on once every hour for 20 minutes each time until the hydrothermal reactor is taken out of the oven;
[0012] (3) Pour out all the materials in the hydrothermal reactor and filter them, dry the filter residue, and transfer it to a planetary mill. Use zirconia balls of different sizes, and mix the mixture with zirconia balls at a weight ratio of 1:6 to 10. After 20-60 minutes of nodularity, take out the mixture;
[0013] (4) The ground mixture is passed through an 800-mesh vibrating screen, the screened material is loaded into a material trough, and placed in a static muffle furnace at 510-550° C. for 5-8 hours, and then heated to 700-770° C. for 5-8 hours at a heating rate of 3° C. / min, and naturally cooled to room temperature to obtain lithium cobalt manganese oxide.
[0014] (5) The obtained lithium cobalt manganese oxide is made into a soft-pack lithium-ion battery.
[0015] Preferably, the lithium source of the present invention is selected from lithium hydroxide or lithium carbonate.
[0016] Preferably, the cobalt source of the present invention is cobalt hydroxide or cobalt tetroxide.
[0017] Preferably, the manganese source of the present invention is manganese acetate or manganese citrate.
[0018] Preferably, the molar ratio of Co to Mn in the lithium cobalt manganese oxide of the present invention is 1:1.2-3.
[0019] Preferably, the additive of the present invention is F127 surfactant.
[0020] Preferably, the dispersant of the present invention is isopropanol or ethylene glycol.
[0021] The invention discloses an application of the lithium cobalt manganese oxide in the preparation of lithium ion batteries.
[0022] In summary, due to the adoption of the above technical solution, the present invention has the following beneficial effects:
[0023] 1. The present invention adopts a hydrothermal-high temperature solid phase method to prepare lithium cobalt manganese oxide battery materials, and simultaneously adopts ultrasonic treatment accompanied by a hydrothermal method to prepare a precursor, thereby reducing or avoiding the problem of particle agglomeration in the preparation process of the precursor, so as to achieve the purpose of stabilizing the particle size and reducing the migration distance of lithium ions, so as to stabilize the performance of the later battery and improve the battery cycle performance.
[0024] 2. The present invention adopts a large proportion of mixing of manganese source and cobalt source. The large proportion of cobalt source can ensure that the battery capacity is relatively high, and the large proportion of manganese also ensures the safety of the battery. Therefore, the comprehensive performance of the lithium cobalt manganese oxide in this scheme is better than that of pure lithium cobalt oxide and pure lithium manganese oxide batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Comparative curve of cycle performance of batteries with various cathode materials in the present invention;
[0026] Figure 2 Photos of the battery status of the overcharge test comparison of the batteries made of various positive electrode materials in the present invention;
[0027] Figure 3 Photos of the battery status of the short-circuit test comparison of the batteries made of various positive electrode materials in the present invention;
[0028] Figure 4 SEM images of the precursors of the embodiments of the present invention. DETAILED DESCRIPTION
[0029] In order to express the present invention more clearly, the present invention is further described below through specific examples.
[0030] Example 1
[0031] The method for preparing lithium cobalt manganese oxide of the present invention comprises the following steps:
[0032] (1) The chemical formula of the lithium cobalt manganese oxide material is LiCo 0.455 Mn 0.545 O2, lithium hydroxide, cobalt hydroxide, and manganese acetate are added in a molar ratio of 1:0.227:0.182, and isopropyl alcohol and F127 surfactant are added at the same time, and the above materials are mixed together to form a mixture, and the mixture is transferred into a planetary mill, and zirconium oxide balls of different sizes are used. The mixture and the zirconium oxide balls are proportioned according to a weight ratio of 1:6, and the mixture is taken out after 20 minutes of nodular graphite;
[0033] (2) The ground mixture is transferred into a hydrothermal reactor, the hydrothermal reactor is placed into an ultrasonic disperser, and then the ultrasonic disperser and the hydrothermal reactor are placed into a high-temperature oven. The heating rate of the oven is 1.5°C / min, and the maximum temperature of the oven is set to 180°C. After the temperature reaches the maximum temperature, it is kept warm for 10 hours. The ultrasonic disperser is turned on once every hour for 20 minutes each time until the hydrothermal reactor is taken out of the oven;
[0034] (3) Pour out all the materials in the hydrothermal reactor and filter them, dry the filter residue, and transfer it to a planetary mill. Use zirconia balls of different sizes, and mix the mixture with zirconia balls at a weight ratio of 1:6. Take out the mixture after 20 minutes of nodularity. Figure 4 shown.
[0035] (4) The ground mixture is passed through an 800-mesh vibrating screen, the screened material is loaded into a material trough, and placed in a static muffle furnace at 510° C. for 5 h, then heated to 700° C. for 5 h at a heating rate of 3° C. / min, and naturally cooled to room temperature to obtain lithium cobalt manganese oxide.
[0036] Example 2
[0037] The method for preparing lithium cobalt manganese oxide of the present invention comprises the following steps:
[0038] (5) The chemical formula of the lithium cobalt manganese oxide material is LiCo 0.25 Mn 0.75 O2, lithium hydroxide, cobalt hydroxide, and manganese acetate are added in a molar ratio of 1:0.125:0.25, and isopropyl alcohol and F127 surfactant are added at the same time, and the above materials are mixed together to form a mixture, and the mixture is transferred into a planetary mill, and zirconium oxide balls of different sizes are used. The mixture and the zirconium oxide balls are proportioned according to a weight ratio of 1:6, and the mixture is taken out after 60 minutes of nodular graphite;
[0039] (6) The ground mixture is transferred into a hydrothermal reactor, the hydrothermal reactor is placed into an ultrasonic disperser, and then the ultrasonic disperser and the hydrothermal reactor are placed into a high-temperature oven. The heating rate of the oven is 3.0°C / min, and the maximum temperature of the oven is set to 180°C. After the temperature reaches the maximum temperature, it is kept warm for 20 hours. The ultrasonic disperser is turned on once every hour for 20 minutes each time until the hydrothermal reactor is taken out of the oven;
[0040] (7) Pour out all the materials in the hydrothermal reactor and filter them, dry the filter residue, and transfer it to a planetary mill. Use zirconia balls of different sizes, and mix the mixture and zirconia balls at a weight ratio of 1:6. Take out the mixture after 60 minutes of nodularity.
[0041] The ground mixture was passed through an 800-mesh vibrating screen, the screened material was loaded into a material trough, and placed in a static muffle furnace at 550°C for 8 hours, then heated to 770°C for 8 hours at a heating rate of 3°C / min, and naturally cooled to room temperature to obtain lithium cobalt manganese oxide.
[0042] Example 3
[0043] The method for preparing lithium cobalt manganese oxide of the present invention comprises the following steps:
[0044] (8) The chemical formula of the lithium cobalt manganese oxide material is LiCo 0.20 Mn 0.8 O2, lithium hydroxide, cobalt hydroxide, and manganese acetate are added in a molar ratio of 1:0.1:0.267, and isopropyl alcohol and F127 surfactant are added at the same time, and the above materials are mixed together to form a mixture, and the mixture is transferred into a planetary mill, and zirconium oxide balls of different sizes are used. The mixture and the zirconium oxide balls are proportioned according to a weight ratio of 1:6, and the mixture is taken out after 40 minutes of nodular graphite;
[0045] (9) The ground mixture is transferred into a hydrothermal reactor, the hydrothermal reactor is placed into an ultrasonic disperser, and then the ultrasonic disperser and the hydrothermal reactor are placed into a high-temperature oven. The heating rate of the oven is 2.0°C / min, and the maximum temperature of the oven is set to 180°C. After the temperature reaches the maximum temperature, it is kept warm for 15 hours. The ultrasonic disperser is turned on once every hour for 20 minutes each time until the hydrothermal reactor is taken out of the oven;
[0046] (10) Pour out all the materials in the hydrothermal reactor and filter them, dry the filter residue, and transfer it to a planetary mill. Use zirconia balls of different sizes, and mix the mixture and zirconia balls at a weight ratio of 1:6. Take out the mixture after 40 minutes of nodularity.
[0047] The ground mixture was passed through an 800-mesh vibrating screen, the screened material was loaded into a material trough, and placed in a static muffle furnace at 530°C for 7 hours, then heated to 750°C for 6 hours at a heating rate of 3°C / min, and naturally cooled to room temperature to obtain lithium cobalt manganese oxide.
[0048] Verification Example
[0049] The lithium cobalt manganese oxide of Example 1 was used as the positive electrode of the battery to make a battery. At the same time, commercially available lithium cobalt oxide and lithium manganese oxide were used as the positive electrode to make batteries of the same specifications for testing.
[0050] 1. Discharge capacity ratio analysis:
[0051] Battery model 604567-2000mAh soft-pack lithium-ion battery, specific test data are as follows Table 1:
[0052] Table 1 Comparative analysis of rate discharge capacity of batteries with different cathode material systems
[0053]
[0054] As can be seen from Table 1, the discharge capacity of the cobalt manganese oxide lithium battery of Example 1 is not much different from that of lithium cobalt oxide, and the charge-discharge capacity ratio is also very small, especially in the case of small current discharge, which is basically the same as that of lithium cobalt oxide. However, the overall discharge capacity and charge-discharge capacity ratio are much improved compared with the lithium manganese oxide battery, especially in the case of large current, the charge-discharge capacity ratio is increased by 9.0%, which also ensures the capacity improvement of the battery.
[0055] 2. Comparative analysis of cycle performance:
[0056] The batteries with the three positive electrode materials were tested for 500 cycles of charge and discharge at 1.0C to analyze their cycle life. Figure 1 As shown in Table 2, the capacity retention rates after 500 cycles are as follows:
[0057] Table 2 Comparison of capacity retention after 500 cycles of different cathode material systems
[0058] Cathode material type 1.0C discharge capacity retention rate Lithium manganate 70.86% Lithium cobalt manganese oxide 89.58% Lithium cobalt oxide 91.99%
[0059] From Table 2 and Figure 1 It can be seen that the cycle performance of the cobalt manganese oxide lithium battery of Example 1 is close to that of the cobalt oxide lithium battery. After 500 cycles of charge and discharge at 1.0C, the cycle performance retention rate of the cobalt manganese oxide lithium battery is nearly 19% higher than that of the manganese oxide lithium battery.
[0060] 3. Safety performance comparison
[0061] (1) Overshoot test: see Figure 2As shown, when the 3C current is overcharged to 4.6V, neither the lithium manganese oxide battery nor the cobalt manganese oxide battery of Example 1 will catch fire, while the cobalt oxide battery will catch fire, indicating that the cobalt manganese oxide battery of Example 1 has a very good overcharge safety performance.
[0062] (2) Short circuit test: After standard charging, connect the positive and negative electrodes with a wire with an internal resistance of less than 50mΩ, monitor the temperature change of the battery, and stop the test when the temperature drops about 10℃ lower than the peak value. Judgment criteria: no fire, no explosion, and the surface temperature does not exceed 150℃. Figure 3 As shown, the lithium manganese oxide battery and the cobalt manganese oxide battery of Example 1 did not catch fire or explode, while one of the cobalt oxide batteries caught fire, exploded and burned. Therefore, it can be determined that the cobalt manganese oxide of Example 1 can meet the short-circuit test safety standard of lithium manganese oxide.
[0063] In summary, the hydrothermal-high temperature solid phase method is used to prepare lithium cobalt manganese oxide battery materials, and ultrasonic treatment is used together with the hydrothermal method to prepare the precursor. The particle dispersion is good, and the particle agglomeration is reduced, so that the material can give full play to its performance, reduce the resistance of the lithium ion channel, and better exert the electrical performance. The battery with lithium cobalt manganese oxide positive electrode material prepared by it can basically meet the electrical performance requirements of lithium cobalt oxide system batteries, and the safety performance of the battery is safer than that of lithium cobalt oxide because it contains manganese.
Claims
1. A method for preparing lithium cobalt manganese oxide, characterized in that: The following steps are involved: (1) The chemical formula of the lithium cobalt manganese oxide material is shown in formula (I), LiCoxMn1-xO2; (I) Among them, x>0, 1>1-x>0; The lithium source, cobalt source and manganese source, additives and dispersants are mixed together to form a mixture, and the mixture is transferred into a planetary mill. Zirconia balls of different sizes are used. The mixture and the zirconium oxide balls are mixed at a weight ratio of 1:6 to 10. The mixture is taken out after 20-60 minutes of nodularity. (2) The ground mixture is transferred into a hydrothermal reactor, the hydrothermal reactor is placed into an ultrasonic disperser, and then the ultrasonic disperser and the hydrothermal reactor are placed into a high-temperature oven. The heating rate of the oven is 1.5-3°C / min, and the maximum temperature of the oven is set to 180°C. After the temperature reaches the maximum temperature, it is kept warm for 10-20 hours. The ultrasonic disperser is turned on once every hour for 20 minutes each time until the hydrothermal reactor is taken out of the oven; (3) Pour out all the materials in the hydrothermal reactor and filter them, dry the filter residue, and transfer it to a planetary mill. Use zirconia balls of different sizes, and mix the mixture with zirconia balls at a weight ratio of 1:6 to 10. After 20-60 minutes of nodularity, take out the mixture; (4) passing the ground mixture through a vibrating screen of 800 mesh, loading the screened material into a material trough, placing it in a static muffle furnace at 510-550° C. for 5-8 hours, then heating it to 700-770° C. for 5-8 hours at a heating rate of 3° C. / min, and cooling it naturally to room temperature to obtain lithium cobalt manganese oxide; (5) The obtained lithium cobalt manganese oxide is made into a soft-pack lithium-ion battery.
2. The method for preparing lithium cobalt manganese oxide according to claim 1, characterized in that: The lithium source is selected from lithium hydroxide or lithium carbonate.
3. The method for preparing lithium cobalt manganese oxide according to claim 1, characterized in that: The cobalt source is cobalt hydroxide or cobalt tetroxide.
4. The method for preparing lithium cobalt manganese oxide according to claim 1, characterized in that: The manganese source is manganese acetate or manganese citrate.
5. The method for preparing lithium cobalt manganese oxide according to claim 1, characterized in that: The molar ratio of Co to Mn in the lithium cobalt manganese oxide is 1:1.2-3.
6. The method for preparing lithium cobalt manganese oxide according to claim 1, characterized in that: The additive is F127 surfactant.
7. The method for preparing lithium cobalt manganese oxide according to claim 1, characterized in that: The dispersant is isopropanol or ethylene glycol.
8. Use of the lithium cobalt manganese oxide as claimed in claims 1 to 7 in the preparation of lithium ion batteries.