Phase change material as well as preparation method and application thereof

By using hollow glass microbeads and negative pressure-ultrasonic treatment technology to improve the adsorption rate of phase-change paraffin and adding copper powder to the concrete, the problem of insufficient adsorption rate and thermal conductivity of existing phase-change energy storage concrete is solved, and the further development is achieved. Efficient temperature regulation and energy utilization.

CN118978357AActive Publication Date: 2024-11-19HUNAN INSTITUTE OF ENGINEERING

Patent Information

Application Number
CN202411466099.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-19
Estimated Expiration
2044-10-21

AI Technical Summary

Technical Problem

The existing phase change energy storage concrete has shortcomings in adsorption rate and leakage rate, and the process of wrapping phase change materials is complex and toxic, which affects its application effect.

Method used

Hollow glass microbeads are used as the carrier to improve the adsorption rate of phase-changed paraffin by negative pressure immersion and pressurization-ultrasound treatment, and copper powder is added to the concrete to improve thermal conductivity and mechanical properties.

Benefits of technology

It significantly improves the adsorption rate of phase change materials and the thermal conductivity and mechanical properties of concrete, improves the temperature fluctuation regulation ability and energy utilization rate, and reduces the compressive strength loss of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention relates to the technical field of concrete, in particular to a phase change material and a preparation method and application thereof. The phase change material is prepared from the following raw materials in parts by weight: 155 to 165 parts of phase change paraffin and 45 to 50 parts of hollow glass beads. According to the invention, the glass beads are used as a carrier to load the phase change paraffin, and after negative pressure soaking, the adsorption rate of the phase change paraffin can be obviously increased by adopting a method of combining pressurized adsorption and ultrasonic concussion technologies. According to the concrete prepared by replacing part of conventional fine aggregate with the phase-change material, on one hand, the concrete can absorb external temperature at high temperature and release heat to the environment at low temperature, and has the advantages of reducing indoor temperature fluctuation, improving the comfort level of the indoor environment, improving the energy utilization rate and the like; and on the other hand, the unique spherical appearance of the phase change material prepared by the method can achieve a ball bearing effect similar to that of fly ash, friction among aggregates can be reduced, and the fluidity and strength of concrete are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of concrete, and in particular to a phase change material and a preparation method thereof, and application of the phase change material in self-compacting phase change energy storage concrete. Background Art

[0002] Concrete is a basic engineering material. The purpose of energy saving is achieved by preparing a special concrete. Its research and development direction is mainly to add other materials to give concrete the special property of storing heat energy to prepare phase change energy storage concrete. In order to expand the application conditions of concrete and develop functional concrete from single function to multi-functional concrete, self-compacting phase change energy storage concrete has been developed on the basis of phase change energy storage concrete. Self-compacting phase change energy storage concrete is a multi-functional concrete with many characteristics such as heat storage, room temperature regulation, hydration heat control, self-compacting, etc., thereby improving the thermal insulation of the wall, such as the phase change energy storage concrete wall for thermal insulation prepared by the prior art CN2022104444044.

[0003] Prior art CN1080173538A discloses a phase-change self-insulating ceramsite foam concrete. The invention first uses porous ceramsite as a carrier, and prepares modified ceramsite by loading paraffin and palmitic acid through a vacuum adsorption method, wherein the ceramsite is a particle of 80-100 mesh, and then uses modified ceramsite and cement as the main raw materials, and glass fiber as a plasticizer, and the raw materials are premixed and mechanically foamed to obtain a phase-change self-insulating ceramsite foam concrete. Although the obtained ceramsite foam concrete has a heat-insulating effect, it does not effectively slow down the temperature fluctuation in the room, the thermal conductivity of the concrete is significantly reduced, and the phase change cycle process cannot be carried out quickly. The patent uses porous ceramsite as a carrier, and encapsulates the phase change material through a vacuum adsorption method to achieve the effect of preliminary encapsulation, but the phase change paraffin adsorption rate and leakage rate still need to be improved.

[0004] Prior art CN 116854432 A discloses a high-strength antifreeze macroporous recycled concrete and its preparation method and application. The raw materials of the macroporous concrete include the following components: 30-50 parts by weight of cement, 2-4.5 parts by weight of fly ash, 130-165 parts by weight of recycled concrete coarse aggregate, 10-16 parts by weight of antifreeze agent, 21-25 parts by weight of glass particles, 13-18 parts by weight of carbon black or iron black, 2-3.5 parts by weight of plastic fiber filaments, and 11-17 parts by weight of mixing water. Wherein: the antifreeze agent is a particle formed by a solid phase change energy storage material core and an asphalt layer coated on its surface, and the asphalt layer is doped with a metal thermal conductor, rubber powder and cement powder, and the phase change energy storage material is paraffin and / or sodium thiosulfate. The above-mentioned high-strength antifreeze macroporous recycled concrete of the invention effectively improves the strength and antifreeze ability of the macroporous concrete prepared with recycled concrete aggregate, and improves the service life of this type of solid waste macroporous concrete. However, the invention adds solid glass beads, which cannot improve the phase change performance in order to increase the surface light transmittance of the concrete. Moreover, the phase change energy storage material of the invention is wrapped with asphalt as the core, and the wrapping process is complicated and toxic gas is discharged during the process, which is very dangerous. Summary of the invention

[0005] The object of the present invention is to provide a phase change material with good heat storage performance, a preparation method thereof and an application thereof in self-compacting phase change energy storage concrete.

[0006] In order to achieve the above object, the technical solution of the present invention is as follows: A phase change material, whose raw materials include, by weight: 155-165 parts of phase change paraffin wax and 45-50 parts of hollow glass microspheres.

[0007] In a preferred embodiment, the chemical composition of the hollow glass microspheres includes, by weight, 50-90 parts of SiO2, 10-50 parts of Al2O3, 5-10 parts of K2O, 1-10 parts of CaO and 0-12 parts of B2O3.

[0008] In a preferred embodiment, the phase change temperature of the phase change paraffin is 28°C.

[0009] In a preferred embodiment, the thermal conductivity of the phase change paraffin is 0.1-0.3 W / m·K, the latent heat of phase change is 200-240 J / g, and the density (solid / liquid) is 0.77-0.88 / cm 3 , specific heat capacity is 1.5-2.5KJ / Kg·K.

[0010] In a preferred embodiment, the true density of the hollow glass microspheres is 0.2-0.4 g / cm 3, bulk density is 0.12-0.24g / cm 3 , thermal conductivity is 0.02-0.06W / m·K, and the moisture content is less than 0.3%.

[0011] In a preferred embodiment, the particle size of the hollow glass microspheres is 0.12-2.28 mm.

[0012] The internal space of hollow glass microspheres that are too small is judged by the adsorption rate of phase-change wax. If the particle size of the hollow glass microspheres is too small, they cannot adsorb enough phase-change wax. If the particle size is too large, the adsorbed phase-change wax will overflow and cause the concrete to be uneven and the performance to deteriorate.

[0013] In a preferred embodiment, the compressive strength of the hollow glass microspheres is 3-120 MPa.

[0014] The greater the compressive strength of the hollow glass microspheres, the smaller the strength loss of the concrete caused by the prepared phase change aggregate replacing the phase change material. However, considering the adsorption rate of the phase change material, the effect is better when the compressive strength is 30-120Mpa.

[0015] There is a certain correlation between the density, particle size and compressive strength of hollow glass microspheres. The wall thickness of the microspheres has a certain influence on the parameters. In general, the larger the particle size, the larger the volume of the sphere, the smaller the density of the microspheres, and the lower the compressive strength; conversely, the smaller the particle size, the greater the density of the microspheres, and the higher the compressive strength. Therefore, under normal circumstances, low-density products have larger particle sizes and lower strength; high-density products have smaller particle sizes and higher strength. Particle size distribution also has a certain influence on compressive strength. Generally, products with narrow particle size distribution have higher compressive strength and also make the composite material have better performance.

[0016] In a preferred embodiment, the phase change temperature of the phase change material is 23-27°C.

[0017] The present invention also claims protection for a method for preparing the phase change material, comprising the following steps: drying the hollow glass microspheres, placing them in a closed environment for vacuuming, adding a paraffin solution until the hollow glass microspheres are completely immersed, placing them in a closed environment for standing for 20-40 minutes, and then performing multiple pressurization-ultrasonic treatments; the pressurization-ultrasonic treatment is: pressurizing the material after standing for 5-15 minutes, then taking out the material and performing ultrasonic vibration for 5-15 minutes.

[0018] In a preferred embodiment, the paraffin solution is a mixed solution in which the mass ratio of phase change paraffin to dispersant is 1:0.02-0.05.

[0019] In a preferred embodiment, the dispersant is polyvinyl alcohol.

[0020] Polyvinyl alcohol can be used as a dispersant on the one hand, and has a defoaming effect on the other hand.

[0021] In a preferred embodiment, the molecular weight of the polyvinyl alcohol is 2000-15000.

[0022] In a preferred embodiment, the temperature of the paraffin solution is 40-50°C.

[0023] In a preferred embodiment, the pressurized pressure is 0.2-0.5 MPa.

[0024] If the pressure is too small, the phase-change paraffin will not be able to completely enter the internal space and the adsorption rate of the phase-change paraffin will be too low; if the pressure is too large, some of the glass beads will be broken.

[0025] In a preferred embodiment, the frequency of the ultrasonic oscillation is 20-70 kHz.

[0026] In a preferred embodiment, the multiple pressurization-ultrasonic treatments are performed 2-3 times on the material after being left to stand.

[0027] In a preferred embodiment, the hollow glass microspheres are screened before drying, and the screening comprises the following steps: Soak the hollow glass microbeads in water for 20-28 hours, stirring every 2 hours; then take out the glass microbeads floating in the middle and upper layers and dry them; then place the dried glass microbeads in a closed environment and evacuate them; then add water; continue to place them in a closed environment and evacuate them for 5-10 minutes; then continue to add water and stir; then let them stand for 10-12 hours; then take out the hollow glass microbeads in the lower layer and dry them to obtain hollow glass microbeads as carriers.

[0028] Hollow glass beads screening is to select intact glass beads by density. The first step is to soak them in water. The intact glass beads have air inside and are less dense than water, so they are in the upper layer of water, while the broken glass beads have a higher density than water and are in the lower layer. The second step is to add water after vacuum. The upper glass beads have no pores, so water does not enter the inside. The inside is air and has a lower density than water. The porous glass beads have water inside, and their density is greater than that of the upper glass beads. Therefore, this method can be used to remove broken glass beads or glass beads without pores.

[0029] Based on the same inventive concept, the present invention also claims to protect the use of the phase change material in preparing self-compacting phase change energy storage concrete.

[0030] Based on the same inventive concept, the present invention also claims protection for a concrete comprising the above-mentioned phase change material.

[0031] In a preferred embodiment, the concrete comprises, by weight: 200-280 parts of water, 500-600 parts of cement, 1000-1200 parts of coarse aggregate, 500-600 parts of fine aggregate, 6-107 parts of the above-mentioned phase change material, 20-25 parts of copper powder, 5-15 parts of water reducer, and 8-12 parts of defoamer.

[0032] In a preferred embodiment, the coarse aggregate is river sand with a particle size of 6-9 mm.

[0033] In a preferred embodiment, the fine aggregate is quartz sand.

[0034] In a preferred embodiment, the particle size of the fine aggregate is not greater than 0.075 mm.

[0035] In a preferred embodiment, the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0036] In a preferred embodiment, the defoaming agent is a polyether defoaming agent.

[0037] Based on the same inventive concept, the present invention also claims a method for preparing the concrete, comprising the following steps: S1. Soak the coarse aggregate, quartz sand, phase change material and copper powder in water for 1-3 hours respectively, take them out, wipe them dry, and obtain pretreated raw materials; S2, the water is divided into two parts, a dispersant and a water reducing agent are added to one part to obtain solution 1; a defoaming agent is added to the other part to obtain solution 2; S3, mixing the pretreated quartz sand, the pretreated copper powder, the pretreated phase change material and cement, adding the solution 1 and stirring, then adding the pretreated coarse aggregate, and slowly adding the solution 2, stirring again for 5-10 minutes; obtaining the concrete.

[0038] The defoamer needs to be dispersed in water first to prepare solution 2 before adding it into the system, otherwise it will be dispersed unevenly.

[0039] The method of using the concrete is as follows: pouring the mixed concrete into a mold, and then transferring the mold to a curing box with appropriate humidity and temperature for curing. After the concrete slurry solidifies and forms, demolding and repairing the mold are performed, and after demolding, the sample is placed in a curing box for curing, and after the curing is completed, a glass microsphere self-compacting concrete test block with phase change energy storage is obtained.

[0040] Based on the same inventive concept, the present invention also claims protection for a concrete wall, comprising the concrete.

[0041] A concrete wall comprises an outer phase change wallboard layer, a foam concrete insulation layer, an inner phase change wallboard layer and a plaster mortar layer stacked in sequence, wherein the outer phase change wallboard layer and the inner phase change wallboard layer are both made of the concrete.

[0042] The present invention provides a multifunctional concrete with significantly improved heat storage performance, thermal conductivity and mechanical properties, and excellent comprehensive performance. The concrete uses modified glass microspheres as phase change materials to provide heat storage performance. The applicant has developed a phase change aggregate with the best comprehensive performance through in-depth research and experiments to replace quartz sand as a phase change material. Hollow glass microspheres have physical characteristics such as low density, low thermal conductivity, low dielectric constant, high compressive strength, high melting point, low water absorption, good fluidity, and good corrosion resistance. The phase change composite material prepared using hollow glass microspheres as a substrate not only improves its workability, reduces its thermal conductivity, and increases its latent heat of phase change, but also helps to improve the mechanical properties of concrete. Although the compressive strength of the concrete will be slightly reduced due to the low compressive strength of the material, it still meets the concrete design specifications. The present invention uses copper powder as an external additive to improve the thermal conductivity and mechanical properties of concrete. During preparation, the copper powder and the coarse phase change material are pre-wetted. Then add a water reducer and a defoamer to improve the working performance of the concrete.

[0043] Compared with the prior art, the present invention has the following beneficial effects: (1) The glass microbeads obtained by repeated screening of the present invention have the physical properties of light weight and high strength, and their compressive strength is 3-120MPa, and their porosity can reach 90%. Their compressive strength increases with the decrease of particle size. The compressive strength of glass microbeads with a particle size of 0.12-2.28mm can reach 120MPa. The glass microbeads obtained by repeated screening have a high porosity and can absorb more phase change paraffin, and their porosity can reach more than 90%. Compared with porous ceramsite, whose compressive strength can only reach 30MPa at most and whose porosity can only reach 70% at most, glass microbeads have more superior comprehensive performance.

[0044] (2) The present invention uses glass microspheres as carriers to load phase-change paraffin wax, and after negative pressure immersion, a method combining pressurized adsorption and ultrasonic oscillation technology is used. After negative pressure treatment, the gas inside the glass microspheres is discharged, so that the phase-change paraffin wax can better adsorb on the inner wall of the glass microspheres without generating bubbles. Then, pressurization is used to force the phase-change paraffin wax to enter the interior of the glass microspheres faster and more, and then ultrasonic oscillation technology is used to shake out the residual bubbles, which can increase the adsorption rate of the phase-change paraffin wax. Compared with the direct immersion method, the adsorption rate of the phase-change paraffin wax is increased by 50%-60%, and compared with the single vacuum adsorption method, it is increased by 12%-16%. The improved technology has significantly improved the adsorption rate of the phase-change paraffin wax compared with the original technology.

[0045] (3) The present invention uses phase change aggregates to replace phase change materials as raw materials. On the one hand, the phase change paraffin wax loaded therein can absorb the external temperature at high temperatures and release heat to the environment at low temperatures, which has the advantages of reducing indoor temperature fluctuations, improving indoor environmental comfort, and improving energy utilization. On the other hand, the unique spherical appearance of the phase change aggregate can play a ball bearing effect similar to fly ash, which can reduce friction between aggregates and improve the fluidity and strength of concrete.

[0046] (4) The present invention uses copper powder as an admixture, which can firstly improve the overall thermal conductivity of concrete, so that the phase-change paraffin wax can quickly exchange heat with the surrounding environment. Secondly, adding an appropriate amount of copper powder can make the concrete more compact and improve the strength and working performance of the concrete.

[0047] (5) The present invention adjusts the formula of concrete, increases the sand ratio to 34%, and adds a water reducer and a defoamer as admixtures. The self-compacting concrete with phase change energy storage is obtained, which has the characteristics of simple construction and easy pouring. DETAILED DESCRIPTION

[0048] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0049] Unless otherwise defined, all professional and scientific terms used in the present invention have the same meaning as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. If not otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equal to the recorded content can be applied to the method of the present invention. The preferred implementation methods and materials described in the present invention are for demonstration purposes only. If not otherwise specified, the relevant percentages are weight percentages.

[0050] The raw materials used in the following examples, phase change paraffin (PCM-A-28), have a phase change temperature of 28°C, which is in line with the optimal temperature of the human body, a thermal conductivity of 0.2 W / m·K, a phase change latent heat of 230±10 J / g, and a density (solid / liquid) of 0.77 g / cm 3 The minimum compressive strength of hollow glass microspheres is 3Mpa and the bulk density is 0.12g / cm 3, thermal conductivity is 0.06W / m·K, and moisture content is less than 0.3%. Cement uses P·O 42.5 ordinary Portland cement, which is provided by Shandong Weifang Jiuqi Building Materials Company. Coarse aggregate uses coarse river sand with a particle size of 6-9mm. Fine aggregate uses quartz sand with a particle size of ≤0.075mm. Water is experimental tap water. Dispersant is polyvinyl alcohol, the molecular weight of polyvinyl alcohol is 2000-15000, water reducer is polycarboxylic acid high-performance water reducer, product model is HLX (standard version) of Shanxi Feike New Materials Technology Co., Ltd., defoamer is polyether defoamer, model is FKXP-1 of Shanxi Feike New Materials Technology Co., Ltd.

[0051] The performance test method is as follows: Compression test: The test was carried out on a concrete universal press in the Civil Engineering Materials Laboratory of the School of Civil Engineering, in accordance with the Standard for Test Methods of Mechanical Properties of Ordinary Concrete (GB / T 50081-200). Where: ; F cc —Compressive strength of concrete test block (MPa); F—specimen failure load (N); A—Test piece pressure bearing area (mm 2 ).

[0052] The experimental steps are as follows: Step 1: Place the specimen in front of the testing machine and wipe the surface of the specimen and the upper and lower pressure plates clean.

[0053] Step 2: Use the side of the specimen when it is formed as the pressure-bearing surface, place the specimen on the lower pressure plate or pad of the testing machine, and align the center of the specimen with the center of the lower pressure plate of the testing machine.

[0054] Step 3: Start the testing machine. The surface of the test piece should be in even contact with the upper and lower pressure plates or steel pads.

[0055] Step 4: The test process is continuous and uniform loading, and the loading speed is 0.5Mpa / s.

[0056] Slump and slump spread test: The slump test can evaluate the working performance of concrete, especially fluidity and plasticity. It can also measure the uniformity and stability of the concrete mixture after adding composite materials to ensure that the concrete has good operability during the construction process to meet the construction requirements.

[0057] The slump and slump spread test should be carried out according to the following steps: 1. Wet the slump cone and base plate. There should be no visible water on the inner wall of the slump cone and the base plate. The base plate should be placed on a solid horizontal surface. Place the slump cone in the center of the base plate, and then step on the foot pedal on the side. The slump cone should remain in a fixed position during loading.

[0058] 2. Use a small shovel to evenly load the concrete samples obtained as required into the slump cone in three layers, so that the height of each layer after compaction is about one-third of the height of the slump cone. Use a tamping rod to insert 25 times into each layer. The insertion and tamping should be carried out from the outside to the center along the spiral direction, and each insertion and tamping should be evenly distributed on the cross section. When inserting the concrete at the edge of the tamping cone, the tamping rod can be slightly tilted. When inserting the bottom layer, the tamping rod should penetrate the entire depth. When inserting the second and top layers, the tamping rod should penetrate the current layer to the surface of the next layer. When pouring the top layer, the concrete should be poured to a height above the slump cone mouth. During the insertion and tamping process, if the concrete sinks below the slump cone mouth, it should be added at any time. After the top layer is inserted and tamped, scrape off the excess concrete and smooth it with a trowel.

[0059] 3. After clearing the concrete on the bottom plate of the cone, lift the slump cone vertically and steadily. The lifting process of the slump cone should be completed within 5-10 seconds. The process from starting to load to lifting the slump cone should be carried out uninterruptedly and should be completed within 150 seconds.

[0060] 4. The height difference between the highest point of the concrete specimen before the slump cone is raised and after the slump is the slump value of the concrete. If the concrete collapses or one side is sheared, re-sample it for further measurement. If the above phenomenon still occurs in the second test, it means that the workability of the concrete is poor and it should be recorded for future reference.

[0061] 5. Observe the cohesiveness and water retention of wet concrete. The cohesiveness can be checked by gently tapping the side of the collapsed concrete cone with a tamping shovel. If the cone gradually sinks, it means the cohesiveness is good. If the cone collapses, partially cracks, or has high precipitation, it means the cohesiveness is poor. Water retention is determined by whether there is slurry precipitation from the concrete. If there is no slurry or only a small amount of slurry precipitates from the bottom after lifting, it means the concrete has good water retention.

[0062] 6. When the slump of the concrete mixture is greater than 220mm, use a steel ruler to measure the maximum and minimum diameters of the concrete after expansion. If the difference between the two diameters is less than 50mm, use their arithmetic mean as the slump expansion value; otherwise, the test is invalid. If coarse aggregate is found to be piled in the center or cement slurry is precipitated at the edge, it means that the segregation resistance of this concrete is not good and should be recorded. The slump and slump spread values ​​of concrete mixtures are measured in millimeters and are accurate to 1mm.

[0063] Thermal conductivity test: Use a multifunctional rapid thermal conductivity meter to measure the thermal conductivity of concrete materials. The following are the test steps: Step 1: Check whether the device is in normal working condition and confirm that the power supply, data cable, etc. are connected correctly. Calibrate the device and perform necessary calibration steps according to the device manual.

[0064] Step 2: Prepare the sample according to the specified size and shape, and ensure that the sample surface is smooth and free of contamination. The thickness and size of the sample should meet the measurement requirements of the equipment.

[0065] Step 3: Ensure that the sample is in close contact with the temperature sensor. If necessary, use thermal grease or other materials to improve contact.

[0066] Step 4: According to the sample material and experimental requirements, enter relevant parameters on the control interface of the equipment, such as sample thickness, initial temperature, test time, etc.

[0067] Step 5: Start the device and start the measurement process. The instrument will heat or cool according to the set parameters and record the temperature changes.

[0068] Phase change cycle durability test Place the test block in a constant temperature drying oven and heat it at 40℃ for 2h, then place the test block in a constant temperature curing room at 20℃ for 2h as a cycle, observe the appearance of the test block after 25 and 50 times, and test its compressive strength Mechanical properties were tested by cube axial compressive strength test and flexural strength test to determine its strength after 7 days, 14 days and 28 days. Thermal conductivity test, slump test, apparent density test and freeze-thaw cycle test were used to determine its thermal conductivity, concrete workability, apparent density and strength loss rate of freeze-thaw cycle. Instruments used in the experimental determination process include concrete pressure testing machine, concrete mixer, concrete curing box, electric blast dryer, electronic temperature control electric heating jacket, slump cone, force-enhancing stepless constant speed mixer, multi-function fast thermal conductivity meter, scanning electron microscope, differential scanner, etc.

[0069] Example 1 Take the hollow glass microsphere raw material with a particle size of 0.12-0.84mm and put it into a bucket. Fill it with distilled water and soak it for 24 hours. Stir it with a steel rod every 2 hours. After 24 hours, take the glass microspheres floating on the upper layer in the bucket, and discard the broken glass microspheres on the lower layer. Put the obtained glass microspheres into a constant temperature drying oven for 12 hours, and then put the dried glass microspheres into a vacuum drying kettle. Use a vacuum pump to extract the air in the drying kettle, open the valve, add distilled water to the drying kettle, close the valve, and continue to use a vacuum pump to extract the air in the drying kettle for 5 minutes. During this period, the drying kettle is shaken continuously to make the glass microspheres completely contact with the distilled water. After the end, open the valve again to allow the air to completely enter the drying kettle. Finally, fill the drying kettle with water, stir it with a steel rod and let it stand for 12 hours. After 12 hours, take out the lower layer of glass microspheres in the drying abdomen, drain the water, and put it into a constant temperature drying oven for drying to obtain hollow glass microspheres as a carrier.

[0070] Put the phase change paraffin wax into a beaker, place the beaker in a constant temperature water bath at 40-50°C, and then add a dispersant to obtain a mixed solution. The mass ratio of the phase change paraffin wax to the dispersant is 1:0.05.

[0071] The dried hollow glass microspheres were placed in a beaker, and liquid paraffin mixture was added until the hollow glass microspheres were covered, and the mixture was allowed to stand for 12 hours. The hollow glass microspheres were counted to be 50 g and the phase change paraffin was 160 g. The hollow glass microspheres modified by the direct standing method were then filtered.

[0072] Example 2 The particle size of the hollow glass microspheres was 0.85-1.56 mm. The operation described in Example 1 was repeated to obtain a phase change aggregate.

[0073] Example 3 The particle size of the hollow glass microspheres was 1.57-2.28 mm. The operation described in Example 1 was repeated to obtain a phase change aggregate.

[0074] Example 4 Take the hollow glass microsphere raw material with a particle size of 0.12-0.84mm and put it into a bucket. Fill it with distilled water and soak it for 24 hours. Stir it with a steel rod every 2 hours. After 24 hours, take the glass microspheres floating on the upper layer in the bucket, and discard the broken glass microspheres on the lower layer. Put the obtained glass microspheres into a constant temperature drying oven for 12 hours, and then put the dried glass microspheres into a vacuum drying kettle. Use a vacuum pump to extract the air in the drying kettle, open the valve, add distilled water to the drying kettle, close the valve, and continue to use a vacuum pump to extract the air in the drying kettle for 5 minutes. During this period, the drying kettle is shaken continuously to make the glass microspheres completely contact with the distilled water. After the end, open the valve again to allow the air to completely enter the drying kettle. Finally, fill the drying kettle with water, stir it with a steel rod and let it stand for 12 hours. After 12 hours, take out the lower layer of glass microspheres in the drying abdomen, drain the water, and put it into a constant temperature drying oven for drying to obtain hollow glass microspheres as a carrier.

[0075] Put the phase change paraffin wax into a beaker, place the beaker in a constant temperature water bath at 40-50°C, and then add a dispersant to obtain a mixed solution. The mass ratio of the phase change paraffin wax to the dispersant is 1:0.05.

[0076] Put the dried hollow glass microspheres into a beaker, add the melted paraffin mixture into the beaker until the glass microspheres are completely submerged, and then put it into a vacuum drying kettle. Count the hollow glass microspheres to be 50g, the phase change paraffin to be 160g, and evacuate for 30-40 minutes to remove the internal air and fill the pores of the glass microspheres with the phase change paraffin. Take out the beaker and put it in a sieve to filter out the excess liquid phase change paraffin, and obtain the phase change aggregate with the phase change paraffin adsorbed in the pores.

[0077] Example 5 Take hollow glass microspheres with a particle size of 0.85-1.56 mm, and repeat the operation described in Example 4 to obtain a phase change aggregate.

[0078] Example 6 Take hollow glass microspheres with a particle size of 1.57-2.28 mm, and repeat the operation described in Example 4 to prepare phase change aggregate.

[0079] Example 7 Take the hollow glass microsphere raw material with a particle size of 0.12-0.84mm and put it into a bucket. Fill it with distilled water and soak it for 24 hours. Stir it with a steel rod every 2 hours. After 24 hours, take the glass microspheres floating on the upper layer in the bucket, and discard the broken glass microspheres on the lower layer. Put the obtained glass microspheres into a constant temperature drying oven for 12 hours, and then put the dried glass microspheres into a vacuum drying kettle. Use a vacuum pump to extract the air in the drying kettle, open the valve, add distilled water to the drying kettle, close the valve, and continue to use a vacuum pump to extract the air in the drying kettle for 5 minutes. During this period, the drying kettle is shaken continuously to make the glass microspheres completely contact with the distilled water. After the end, open the valve again to allow the air to completely enter the drying kettle. Finally, fill the drying kettle with water, stir it with a steel rod and let it stand for 12 hours. After 12 hours, take out the lower layer of glass microspheres in the drying abdomen, drain the water, and put it into a constant temperature drying oven for drying to obtain hollow glass microspheres as a carrier.

[0080] Put the phase change paraffin wax into a beaker, place the beaker in a constant temperature water bath at 40-50°C, and then add a dispersant to obtain a mixed solution. The mass ratio of the phase change paraffin wax to the dispersant is 1:0.05.

[0081] Put the dried hollow glass microspheres into a beaker, and use a vacuum drying kettle to suck the hollow glass microspheres for 10-15 minutes, then open the valve, add the liquid mixed solution until the hollow glass microspheres are completely immersed, and the hollow glass microspheres are 50g and the phase change paraffin is 160g. Let it stand for 30 minutes, and then use a vacuum drying kettle to pressurize the internal materials for 10 minutes, take out the materials and perform ultrasonic vibration for 10 minutes. After two cycles of pressure treatment and ultrasonic vibration, filter the obtained materials to obtain phase change aggregate.

[0082] Example 8 The particle size of the hollow glass microspheres was 0.85-1.56 mm. The operation described in Example 7 was repeated to obtain a phase change aggregate.

[0083] Example 9 The particle size of the hollow glass microspheres was 1.57-2.28 mm. The operation described in Example 7 was repeated to obtain a phase change aggregate.

[0084] The compressive strength, thermal conductivity and adsorption rate of the phase change aggregate prepared in the above embodiment were tested, and the results are as follows:

[0085] It can be seen from Table 1 that the modification of glass microspheres, glass microspheres of different particle sizes and different modification processes all have an impact on the adsorption rate, compressive strength and thermal conductivity of the glass microspheres.

[0086] Adsorption rate: By comparing Examples 1, 2, 3 with Examples 4, 5, 6 and Examples 7, 8, 9, it can be clearly seen that the adsorption rates of Examples 2, 5, and 6 are more than 10% higher than those of the other two groups, and it is known that the hollow glass microspheres with a particle size of 0.85-1.56 mm have the highest adsorption efficiency after modification. By comparing 1, 4, 7 with 2, 5, 8 and 3, 6, 9, it can be clearly seen that the use of the construction process of cyclic pressurization for phase change paraffin modification is more efficient than direct static immersion and traditional vacuum adsorption.

[0087] Compressive strength: By comparing Examples 1, 2, 3 with Examples 4, 5, 6 and Examples 7, 8, 9, it can be clearly seen that the compressive strength decreases significantly with the increase of particle size. The strength of glass microspheres with a particle size of 1.57-2.28 mm is too small to meet the basic requirements of the carrier's compressive strength. By comparing 1, 4, 7 with 2, 5, 8 and 3, 6, 9, it can be seen that although the glass microspheres modified by different processes adsorb different phase-change paraffin waxes, their compressive strength does not change much, and the glass microspheres with high adsorption rates have slightly higher compressive strength than the glass microspheres with low adsorption rates.

[0088] Thermal conductivity: By comparing Examples 1, 2, 3 with Examples 4, 5, 6 and Examples 7, 8, 9, it can be clearly seen that the thermal conductivity of Examples 2, 5, 8 is higher than that of the other two groups, and it is known that the hollow glass microspheres with a particle size of 0.85-1.56 mm have the highest thermal conductivity after modification. By comparing 1, 4, 7 with 2, 5, 8 and 3, 6, 9, it can be clearly seen that the phase change paraffin modification using the cyclic pressurization construction process is superior to direct static immersion and traditional vacuum thermal conductivity.

[0089] Example 10 Ceramic clay control group The ceramsite was crushed and sieved to obtain particles of 0.85-1.56 mm, and the operation described in Example 7 was repeated to obtain modified ceramsite.

[0090] Embodiment 11 Solid glass beads control group Solid glass microspheres with a particle size of 0.85-1.56 mm were taken, and the operation described in Example 7 was repeated to obtain modified solid glass microspheres.

[0091] The compressive strength, thermal conductivity and adsorption rate of the phase change aggregate prepared in the above embodiment were tested, and the results are as follows:

[0092] By comparing Example 8 with the solid glass microsphere control group 11, it can be clearly seen that the adsorption efficiency of the modified hollow glass microspheres is much higher than that of the modified solid glass microspheres, and the solid glass microspheres cannot be used as a carrier material for phase-change paraffin. By comparing Example 8 with the ceramsite control group 10, it can be clearly seen that compared with the traditional ceramsite as a carrier material for processing and modification, the hollow glass microspheres have a higher adsorption efficiency for phase-change paraffin.

[0093] By comparing Example 8 with the ceramsite control group 10, it can be clearly seen that compared with the traditional ceramsite used as a carrier material for processing and modification, the strength of the hollow glass microspheres after modification is higher.

[0094] By comparing Example 8 with the solid glass microsphere control group 11, it can be clearly seen that the thermal conductivity of the modified hollow glass microspheres is far better than that of the modified solid glass microspheres. By comparing Example 8 with the ceramsite control group 10, it can be clearly seen that compared with the traditional ceramsite as a carrier material for processing and modification, the thermal conductivity of the modified hollow glass microspheres is better.

[0095] It can be seen that the thermal conductivity of the modified material is linearly related to the adsorption rate, and the thermal conductivity of the carrier material with a high adsorption rate after modification is also relatively good. Through comprehensive tests of compressive strength, thermal conductivity and adsorption rate, it can be seen that in Example 8, the phase change aggregate prepared by the hollow glass microspheres with a particle size of 0.85-1.56 mm using a construction process of repeatedly controlling pressure has more outstanding comprehensive performance.

[0096] Example 12 The screened phase change aggregates are used to replace fine aggregates in different volume proportions and copper powder is added. After treatment, phase change energy storage glass bead self-compacting concrete is prepared, and the preparation process with the optimal ratio is selected through testing.

[0097] Basic formula The composition and content of the concrete in this embodiment are calculated by weight: Raw material mass 533 parts of ordinary Portland cement 537 pieces of sand 1090 pieces of stone 240 parts water Water reducing agent (dispersant) 21.3 parts Defoaming agent 10.66 parts The preparation method comprises the following steps: Step 1: Weigh cement, sand, stone and other raw materials according to the mix ratio.

[0098] Step 2: Divide the weighed water into two parts, add dispersant and water reducer to the first part, and add defoamer to the second part.

[0099] Step 3: Pre-mix cement, sand and stone for 5 minutes, then add the first portion of water and continue stirring until the mixture becomes fine and uniform. Then add the coarse aggregate. At this time, slowly add the second portion of water containing defoaming agent, stir again for 5-10 minutes, and observe its fluidity.

[0100] Step 4: Quickly pour the evenly mixed concrete slurry into the mold, and quickly transfer the concrete slurry with the mold to a curing box with appropriate relative humidity and temperature for curing. After the concrete slurry solidifies and forms, demold and repair the mold. After demolding, place the sample in the curing box for curing. After the curing is completed, a self-compacting concrete test block is obtained.

[0101] Example 13 The composition and content of the concrete in this embodiment are calculated by weight: Raw material mass 533 parts of ordinary Portland cement 456.45 parts of sand 1090 pieces of stone 240 parts water Phase change aggregate (Example 8) 32.72 parts Copper powder 26.65 parts Water reducing agent (dispersant) 21.3 parts Defoaming agent 10.66 parts The preparation method comprises the following steps: Step 1: Take the pre-prepared phase change aggregate by weight, and then weigh other raw materials.

[0102] Step 2: Immerse the coarse and fine aggregates and copper powder in water for 2 hours, take them out and wipe off the surface moisture to obtain the raw materials treated by the pre-wetting method.

[0103] Step 3: Divide the weighed water into two parts, add dispersant and water reducer to the first part, and add defoamer to the second part.

[0104] Step 4: Pre-mix the pre-wetted fine aggregate, copper powder and cement for 5 minutes, then add the first portion of water and continue stirring until the mixture becomes fine and uniform, then add the coarse aggregate, then slowly add the second portion of water containing the defoamer, stir again for 5-10 minutes, and observe its fluidity.

[0105] Step 5: Quickly pour the evenly mixed concrete paste into the mold, and quickly transfer the concrete paste with the mold to a curing box with appropriate relative humidity and temperature for curing. After the concrete paste solidifies and forms, demold and repair the mold. After demolding, place the sample in the curing box for curing. After the curing is completed, a glass bead self-compacting concrete test block with phase change energy storage is obtained.

[0106] Embodiment 14 In this embodiment, on the basis of Embodiment 13, 429.6 parts of fine aggregate and 43.62 parts of phase change aggregate are taken, and the rest remain unchanged.

[0107] Embodiment 15 In this embodiment, on the basis of Embodiment 13, 402.75 parts of fine aggregate and 54.53 parts of phase change aggregate are taken, and the rest remain unchanged.

[0108] Example 16 In this embodiment, on the basis of Embodiment 13, 456.45 parts of fine aggregate, 32.72 parts of phase change aggregate, and the copper powder content are changed to 53.3 parts, while the other contents remain unchanged.

[0109] Embodiment 17 In this embodiment, on the basis of Embodiment 13, 429.6 parts of fine aggregate, 43.62 parts of phase change aggregate, and the copper powder content are changed to 53.3 parts, while the other contents remain unchanged.

[0110] Embodiment 18 In this embodiment, on the basis of Embodiment 13, 402.75 parts of fine aggregate, 54.53 parts of phase change aggregate, and the copper powder content are changed to 53.3 parts, while the other contents remain unchanged.

[0111] Embodiment 19 In this embodiment, on the basis of Embodiment 13, 456.45 parts of fine aggregate, 32.72 parts of phase change aggregate, and the copper powder content are changed to 79.95 parts, while the other contents remain unchanged.

[0112] Embodiment 20 In this embodiment, on the basis of Embodiment 13, 429.6 parts of fine aggregate and 43.62 parts of phase change aggregate are taken, the copper powder content is changed to 79.95 parts, and the other contents remain unchanged.

[0113] Embodiment 21 In this embodiment, on the basis of embodiment 13, 402.75 parts of fine aggregate and 54.53 parts of phase change aggregate are taken, the copper powder content is changed to 79.95, and the other contents remain unchanged.

[0114] Embodiment 22 In this embodiment, on the basis of Embodiment 13, 456.45 parts of fine aggregate and 32.72 parts of phase change aggregate are taken, copper powder is not added, and other aspects remain unchanged.

[0115] The formulations of Examples 12-22 are listed and compared in detail as follows:

[0116] The above examples were tested for compressive strength, thermal conductivity, slump, and freeze-thaw cycle, and the test results are as follows:

[0117] It can be seen from Table 4 that phase change aggregate is used as fine aggregate to replace river sand, and copper powder is used as an external additive. The replacement rate of different phase change aggregates and the amount of copper powder have an impact on the compressive strength, thermal conductivity, and workability of concrete.

[0118] Compressive strength: By comparing Examples 13, 14, 15 with Examples 16, 17, 18 and Examples 19, 20, 21, it can be seen that when the copper powder content is the same, the compressive strength decreases as the replacement rate of the phase change aggregate increases, and the replacement rate is from 20% to 25%, and the compressive strength decreases significantly. By comparing Examples 13, 16, 19 with Examples 14, 17, 20 and Examples 15, 18, 21, it can be found that when the phase change aggregate replacement rate is the same, the greater the copper powder content, the slightly greater the compressive strength.

[0119] Thermal conductivity: The thermal conductivity of the concrete test block is directly related to the replacement rate of the phase change aggregate and the copper powder content. By comparing Examples 13, 14, 15 with Examples 16, 17, 18 and Examples 19, 20, 21, it can be seen that when the copper powder content is the same, the thermal conductivity decreases as the replacement rate of the phase change aggregate increases. By comparing Examples 13, 16, 19 with Examples 14, 17, 20 and Examples 15, 18, 21, it can be found that when the phase change aggregate replacement rate is the same, the greater the copper powder content, the better the thermal conductivity.

[0120] Through comprehensive comparison, it can be seen that after phase change aggregate replaces part of fine aggregate and is doped with copper powder, the concrete has superior compressive strength and excellent workability and better thermal conductivity than traditional concrete, and its overall performance is better than other groups.

[0121] Embodiment 23 The concrete of Example 13 is used to prepare a phase change energy storage concrete wall for thermal insulation, as follows: A phase change energy storage concrete wall for thermal insulation, which is sequentially composed of an outer phase change wallboard layer, a foam concrete thermal insulation layer, an inner phase change wallboard layer and a plaster mortar layer. The outer phase change wallboard layer and the inner phase change wallboard layer are respectively arranged on both sides of the foam concrete thermal insulation layer, and the plaster mortar mixed with phase change material is coated on the inner phase change wallboard layer.

[0122] The material composition of the outer phase change wallboard layer 1 and the inner phase change wallboard layer 3 is the concrete of Example 13. The thickness of the outer phase change wallboard layer is 30 mm, and the thickness of the inner phase change wallboard layer is 20 mm.

[0123] The plaster mortar is sprayed on the inner phase change wallboard layer. The thickness of the plaster mortar layer is approximately between 3-4 mm. The material composition of the plaster mortar includes 5 parts of ordinary Portland cement, 6 parts of sand and 33 parts of water.

[0124] The thickness of the foam concrete insulation layer is 150 mm. The material composition includes 203 parts of ordinary Portland cement, 51 parts of fly ash, 71 parts of water, 3 parts of foaming agent (purchased from Nanjing Jieerda Cleaning Agent Factory, AL-56094631), and 0.3 parts of boric acid.

[0125] The specific heat capacity of the concrete wall measured at 35°C is 1.461KJ / KG·°C, the specific heat capacity measured at 5°C is 1.102KJ / KG·°C, and the thermal conductivity is 0.51W·m·k.

[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A phase change material, It is characterized in that The raw materials include, by weight: 155-165 parts of phase-change paraffin wax and 45-50 parts of hollow glass microspheres; the particle size of the hollow glass microspheres is 0.12-2.28 mm.

2. The phase change material according to claim 1, It is characterized in that The phase change temperature of the phase change material is 23-27°C.

3. The phase change material according to claim 1, It is characterized in that The phase-change paraffin wax has a thermal conductivity of 0.1-0.3 W / m·K, a phase-change latent heat of 200-240 J / g, and a density of 0.77-0.88 / cm 3 , specific heat capacity is 1.5-2.5KJ / Kg·K.

4. The phase change material according to claim 1, It is characterized in that The compressive strength of the hollow glass microspheres is 3-120 MPa.

5. The method for preparing the phase change material according to any one of claims 1 to 4, It is characterized in that The method comprises the following steps: drying the hollow glass microbeads, placing them in a closed environment for vacuuming, adding a paraffin solution until the hollow glass microbeads are completely immersed, placing them in a closed environment for standing for 20-40 minutes, and then performing multiple pressurization-ultrasonic treatments; the pressurization-ultrasonic treatment comprises: pressurizing the material after standing for 5-15 minutes, taking out the material and performing ultrasonic vibration for 5-15 minutes.

6. The preparation method according to claim 5, It is characterized in that The paraffin solution is a mixed solution of phase change paraffin and dispersant in a mass ratio of 1:0.02-0.05; the pressurization pressure is 0.2-0.5Mpa; the frequency of the ultrasonic oscillation is 20-70 kHz; multiple pressurization-ultrasonic treatment means that the material after standing is subjected to pressurization-ultrasonic treatment 2-3 times.

7. The preparation method according to claim 5 or 6, It is characterized in that The hollow glass microspheres are screened before drying, and the screening comprises the following steps: Soak the hollow glass microbeads in water for 20-28 hours, stirring every 2 hours; then take out the glass microbeads floating in the middle and upper layers and dry them; then place the dried glass microbeads in a closed environment and evacuate them; then add water; continue to place them in a closed environment and evacuate them for 5-10 minutes; then continue to add water and stir; then let them stand for 10-12 hours; then take out the hollow glass microbeads in the lower layer and dry them to obtain hollow glass microbeads as carriers.

8. A concrete, It is characterized in that The concrete comprises the phase change material according to any one of claims 1 to 4.

9. The concrete according to claim 8, It is characterized in that The concrete comprises, by weight: 200-280 parts of water, 500-600 parts of cement, 1000-1200 parts of coarse aggregate, 500-600 parts of fine aggregate, 6-107 parts of the phase change material according to any one of claims 1-4, 20-25 parts of copper powder, 5-15 parts of water reducing agent, and 8-12 parts of defoaming agent.

10. A concrete wall, It is characterized in that It comprises an outer phase change wallboard layer, a foam concrete insulation layer, an inner phase change wallboard layer and a plaster mortar layer stacked in sequence, wherein the outer phase change wallboard layer and the inner phase change wallboard layer are both made of the concrete according to claim 8 or 9.

Citation Information

Patent Citations

  • Fly ash phase change microbead, preparation method thereof and application

    CN102925114A

  • Fair-faced concrete and preparation method thereof

    CN109503066A

  • C25 phase change energy storage concrete with high-titanium slag as phase change carrier and preparation method of concrete

    CN109553354A

  • High-strength concrete and preparation method thereof

    CN109574583A

  • C80 high-strength concrete and preparation method thereof

    CN111410488A

Cited By

  • Lightweight thermal insulation and sound insulation mortar and preparation method thereof

    CN119613146A