Temperature-inhibiting type self-healing concrete anti-cracking waterproof agent and preparation method thereof
By modifying the combination of raw materials such as nano silica, maltodextrin and 3-mercaptoalanine, a temperature-resistant concrete crack-resistant waterproofing agent with self-healing ability is formed, and the problems of concrete cracking and water seepage in the prior art are solved. , achieving efficient hydration heat suppression and waterproofing performance improvement.
Patent Information
- Application Number
- CN202411041626.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
Existing crack-resistant waterproofing agents cannot effectively solve the problems of concrete cracking and seepage, and the waterproofing effect gradually weakens in long-term humid environments, which may have a negative impact on the hardening performance of concrete.
Modified nanosilicon dioxide, modified maltodextrin, sodium metasilicate, 3-mercaptoalanine and other raw materials are grafted through esterification and carboxylic and amino reactions to form a temperature-inhibiting type with self-healing ability. Concrete crack-resistant waterproofing agent reduces the hydration heat rate, improves pore structure, enhances adhesion and waterproofing performance.
Effectively inhibit hydration heat, prevent the occurrence of temperature cracks, improve the durability, waterproofness and crack resistance of concrete, extend service life, and maintain the hydration heat suppression effect in high-temperature environments.
Smart Images

Figure BDA0004972532810000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to a temperature-suppressing self-healing concrete anti-cracking waterproofing agent and a preparation method thereof. Background Art
[0002] With the development of society and the continuous improvement of residents' quality of life, the public has put forward higher requirements for the performance and quality of building materials, especially for the crack resistance, waterproofness and durability of concrete. Concrete cracking is usually caused by the following factors: First, during the hydration and hardening process of concrete, the volume shrinkage and deformation caused by temperature and dryness may cause cracks and water seepage problems, which will significantly reduce the durability of concrete; secondly, the tiny pores distributed inside the concrete are also prone to water seepage under the influence of hydrostatic pressure and capillary action. Long-term water seepage problems will cause serious damage to concrete, mortar and even the entire building structure. Therefore, waterproof performance is crucial to ensuring the quality of the project, and solving the problems of concrete cracking and water seepage has also become a key issue in the field of concrete research.
[0003] In the domestic construction industry, common types of anti-cracking waterproofing agents include higher fatty acids, triethanolamine and ferric chloride. As a commonly used waterproofing material, higher fatty acid compounds can effectively reduce the absorption of water in concrete capillaries. However, as the amount added increases, the strength of the concrete may be affected, and its waterproofing effect will gradually weaken in a long-term humid environment. Triethanolamine and ferric chloride are also commonly used materials to improve the impermeability of concrete, but they have not been able to effectively solve the problem of concrete cracking in the long term. In addition, since the presence of chloride ions may cause steel corrosion, if triethanolamine is used improperly, it may have a negative impact on the later hardening properties of concrete, and its use has been restricted. It can be seen that the existing anti-cracking waterproofing agents often cause some negative effects in actual engineering applications and cannot achieve the expected waterproofing effect.
[0004] Chinese patent CN 113548829 B relates to a concrete intelligent self-repairing waterproof and anti-corrosion compacting agent, comprising the following components: nano silica sol, sodium salt, sodium hydroxide, potassium hydroxide, lithium hydroxide, bactericide, defoamer, emulsifier, and deionized water. The waterproof and anti-corrosion compacting agent solves the problem that the waterproof and anti-corrosion compacting agent in the prior art has poor compacting effect and affects the mechanical properties of concrete. However, it cannot suppress hydration heat well and may cause temperature cracks.
[0005] Therefore, there is an urgent need for a temperature-suppressing self-healing concrete anti-cracking waterproofing agent that has strong crack resistance, excellent waterproofing, and can effectively inhibit hydration heat. Summary of the invention
[0006] In view of the existing technical problems, the purpose of the present invention is to provide a temperature-suppressing self-healing concrete anti-cracking waterproofing agent and a preparation method thereof. The anti-cracking waterproofing agent of the present invention has self-healing ability, can effectively inhibit hydration heat, reduce the hydration heat release rate of concrete, and thus prevent the generation of temperature cracks. At the same time, it can effectively improve the durability, workability and waterproofness of concrete structures, and has good market value.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] On one hand, the present invention provides a temperature-suppressing self-healing concrete anti-cracking waterproofing agent. The anti-cracking waterproofing agent comprises the following raw materials in parts by weight: 10-30 parts of modified nano-silicon dioxide, 15-25 parts of modified maltodextrin, 5-10 parts of sodium metasilicate, 4-8 parts of sodium gluconate, 3-6 parts of modified 3-mercaptoalanine, 3-5 parts of calcium nitrate, 2-4 parts of potassium hydroxide, 1-2 parts of defoaming agent, 1-2 parts of dispersant, and 30-50 parts of water.
[0009] The reaction mechanism and effects of this application are as follows:
[0010] 1. During the hydration process of concrete, the reaction between cement and water will generate a large amount of heat. Especially when constructing large-volume concrete or in high-temperature seasons, this temperature rise will cause cracks. Maltodextrin can reduce the hydration heat release rate and prolong the heat release time of concrete, thereby reducing the temperature peak after cement concrete pouring, reducing cracks caused by temperature changes, and improving the overall stability and durability of the concrete structure. In addition, maltodextrin can improve the pore structure of concrete, increase the density of concrete, and thus improve the impermeability of concrete. The low hygroscopicity of maltodextrin reduces the risk of cracks and damage caused by moisture. However, the hydration heat inhibition effect of maltodextrin will be weakened when the ambient temperature is high (>35°C).
[0011] The present invention introduces glutaric acid groups into maltodextrin molecules through esterification reaction, which can increase the active functional groups of maltodextrin, thereby improving its reactivity and compatibility. The applicant further grafts 2-acrylamide-2-methylpropanesulfonic acid through carboxyl and amino reactions to improve the heat resistance of maltodextrin, so that it can effectively exert its hydration heat inhibition effect at high temperatures. On the other hand, the sulfonic acid group can form a localized hydrated proton domain on the surface of the material. The high proton concentration helps to form short hydrogen bonds, thereby promoting the rapid conduction of protons inside the material, accelerating the migration of water molecules, and reducing the retention of water inside the material, thereby reducing the risk of cracks caused by water evaporation or uneven migration. Moreover, the raw materials will migrate to every corner of the gap with the water molecules, better and faster self-healing tiny cracks, and improving the durability and waterproof and crack resistance of concrete.
[0012] In addition, modified maltodextrin can also cross-link with modified nano-titanium dioxide, making the nano-titanium dioxide more evenly dispersed, better exerting its role, and also improving the stability of the anti-cracking waterproofing agent.
[0013] 2.3-Mercaptoalanine can slow down the shrinkage deformation rate of concrete, effectively prevent cracking and cracking on the concrete surface, improve the compressive strength and wear resistance of concrete, and improve the density and durability of concrete, effectively improve the anti-permeability and waterproof performance of concrete, and extend the service life of concrete; in addition, the thiol group of 3-mercaptoalanine can form a coordination bond with the metal ions in the concrete, thereby enhancing the adhesion of the anti-cracking waterproofing agent to the concrete substrate, and helping to form a more uniform and continuous waterproof layer. However, when the cement hydration reaction releases heat, 3-mercaptoalanine may lose its activity or even denature.
[0014] In the present invention, the amino group of 3-mercaptoalanine attacks the epoxy ring of (R)-benzyloxymethyl oxirane, a nucleophilic addition reaction occurs, and a corresponding modified compound is generated. The active groups of 3-mercaptoalanine can be increased by epoxy modification, and then it can react with calcium carbonate as an effective complexing agent to generate a soluble calcium salt complex. During cement hydration, these calcium salt complexes will naturally penetrate into the interior of the concrete along with the migration of water, and then react with the modified nano-silicon dioxide and sodium metasilicate in the raw materials to form water-insoluble calcium silicate crystals, which can fill the tiny gaps in the concrete, thereby effectively repairing the cracks inside the concrete and improving the overall compactness of the concrete. In this way, the strength of the concrete is enhanced, and the waterproof performance is also significantly improved. In addition, the introduction of (R)-benzyloxymethyl oxirane makes the modified 3-mercaptoalanine have a benzene ring structure, which improves its heat resistance and further improves the hydrophobicity.
[0015] 3. The modified nano silicon dioxide and sodium metasilicate of the present invention can better penetrate deep into the concrete, react chemically with calcium ions in the concrete, generate calcium silicate crystals, and help fill and seal the tiny pores in the concrete, thereby achieving structural densification and pore sealing. The generated crystals can both attract water and repel moisture, and can provide a dual waterproof effect; in addition, they can also penetrate deep into the microscopic pores of the concrete, effectively remove internal dirt and impurities, and discharge them from the surface, thereby maintaining the cleanliness and integrity of the concrete surface.
[0016] In some embodiments, the modified nano-silica is prepared by modifying nano-silica with an unsaturated silane coupling agent.
[0017] Specifically, the preparation method of the modified nano-silicon dioxide comprises the following steps:
[0018] Ⅰ. Add the unsaturated silane coupling agent to a reaction kettle containing a mixed solvent, and stir at a speed of 3000-5000 r / min for 30-40 min to obtain a hydrolysis solution;
[0019] Ⅱ. Take the hydrolysis solution and nano-silica obtained in step Ⅰ and add them to the reactor, heat to 50-60°C, stir at a speed of 3000-5000r / min for 3-4h, wash with anhydrous ethanol 3-4 times, and centrifuge at a speed of 7000-8000r / min for 6-8min to obtain modified nano-silica.
[0020] Preferably, the nano-silicon dioxide is hydrophobic nano-silicon dioxide with a specific surface area of 150-200m 2 / g.
[0021] In some embodiments, the method for preparing the modified maltodextrin comprises the following steps:
[0022] (1) adding maltodextrin, glutaric acid and water into a reaction kettle, mixing and dissolving, then adding a catalyst, stirring, and drying to obtain a mixture;
[0023] (2) pouring the mixture obtained in step (1) into a reaction kettle, heating to 120-180° C., and reacting for 15-40 minutes to obtain an intermediate product;
[0024] (3) dissolving the intermediate product obtained in step (2) in water, then adding anhydrous ethanol, filtering the precipitate, washing, and drying to obtain a modified product;
[0025] (4) Add the modified product obtained in step (3), 2-acrylamide-2-methylpropanesulfonic acid, and water into a reaction kettle, then add a carbodiimide condensing agent and an activator, heat to 60-80° C., and stir the reaction for 6-8 hours to obtain modified maltodextrin.
[0026] In some embodiments, the molar ratio of maltodextrin to glutaric acid in step (1) is 1:(2-6).
[0027] Preferably, the molar ratio of maltodextrin to glutaric acid in step (1) is 1:(3-5).
[0028] Preferably, the DE value of the maltodextrin in step (1) is 5-15.
[0029] Preferably, the drying method in step (3) is hot air drying or vacuum drying.
[0030] In some embodiments, step (2) can also be processed by microwave, and the specific steps are: pouring the mixture obtained in step (1) into a reaction kettle, using a microwave power of 160-800 W, reacting for 20-400 seconds, and obtaining an intermediate product.
[0031] In some embodiments, the molar ratio of the modified product to 2-acrylamide-2-methylpropanesulfonic acid in step (4) is 1:(2-4).
[0032] In some embodiments, the method for preparing the modified 3-mercaptoalanine comprises the following steps:
[0033] S1. Mix 3-mercaptoalanine and water and add them to a reactor, add sodium hydroxide to adjust the pH to alkaline, then add (R)-benzyloxymethyl oxirane dropwise, heat to 50-60°C, and stir to react for 2-3h;
[0034] S2. After the reaction is completed, hydrochloric acid is added to adjust the pH to neutral, the mixture is allowed to stand for stratification, the lower layer is taken, and concentrated by rotary evaporation to obtain modified 3-mercaptoalanine.
[0035] In some embodiments, the molar ratio of 3-mercaptoalanine to (R)-benzyloxymethyl oxirane is (1.1-1.3):1.
[0036] In some embodiments, the dispersant is a polycarboxylate dispersant.
[0037] In some embodiments, the defoaming agent is a silicone defoaming agent.
[0038] Another aspect of the present invention provides a method for preparing a temperature-suppressing self-healing concrete anti-cracking waterproofing agent, comprising the following steps:
[0039] 1. Add modified nano-silicon dioxide, modified maltodextrin, sodium metasilicate, sodium gluconate, modified 3-mercaptoalanine and water into a reaction kettle, stir for 20-30 minutes, add calcium nitrate and potassium hydroxide in sequence, heat to 30-40°C, stir for 5-10 minutes, cool to obtain a mixed substance;
[0040] 2. Mix the defoamer and dispersant, stir for 5-10 minutes, add the mixed substance obtained in step 1, heat to 30-40° C., stir for 20-30 minutes, and obtain the anti-cracking waterproofing agent.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] 1. The anti-cracking waterproofing agent of the present invention has self-healing ability, can effectively inhibit hydration heat, reduce the hydration heat release rate of concrete, and thus prevent the generation of temperature cracks. At the same time, it can effectively improve the durability, workability and waterproofness of concrete structures.
[0043] 2. The anti-cracking and waterproofing agent of the present invention is an aqueous liquid with good permeability and can better play the role of waterproofing and anti-cracking.
[0044] 3. The modified maltodextrin of the present invention is heat-resistant and has many active functional groups, which improves its reaction activity and compatibility and effectively exerts its hydration heat inhibition effect; at the same time, the introduced sulfonic acid group can reduce the risk of cracks caused by water evaporation or uneven migration, and the raw materials will migrate to every corner of the gap with the water, better and faster self-healing tiny cracks, thereby improving the durability and waterproof and crack resistance of concrete.
[0045] 4. The modified 3-mercaptoalanine in the present invention can effectively repair cracks inside concrete and improve the overall density and waterproof performance of concrete. DETAILED DESCRIPTION
[0046] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, rather than to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0047] According to the ratios of the raw materials and the preparation methods specified in the following examples and comparative examples, various anti-cracking waterproofing agents were prepared.
[0048] In order to facilitate those skilled in the art to implement the present invention, some raw material manufacturers of the embodiments and comparative examples are described as follows:
[0049] Hydrophobic nano-silica: purchased from Nanjing Tianxing New Materials Co., Ltd., model TSP-L20, with a specific surface area of 200m 2 / g;
[0050] Maltodextrin: purchased from Hubei Qibajiu Chemical Co., Ltd., DE value 8-10;
[0051] Polycarboxylate dispersant: purchased from Shandong Yuqian Chemical Co., Ltd., model LY-600;
[0052] Organic silicon defoamer: purchased from Tianjin Shengsheng Technology Development Co., Ltd.; model SDF-043;
[0053] Other raw materials are not specially specified and can be purchased from the market.
[0054] Preparation Example 1
[0055] The preparation method of modified hydrophobic nano-silica comprises the following steps:
[0056] Ⅰ. Add 0.6 g of vinyltrimethoxysilane to a reactor containing a mixed solvent (2 ml of deionized water and 20 ml of ethanol), and stir at a speed of 5000 r / min for 30 min to obtain a hydrolysis solution;
[0057] Ⅱ. Add the hydrolysis solution obtained in step Ⅰ and 5g of hydrophobic nano-silica into the reactor, heat to 50°C, stir at a speed of 3000r / min for 3h, wash with anhydrous ethanol 3 times, centrifuge at a speed of 8000r / min for 6min, take out the powder, and dry it at 80°C for 4h to obtain modified nano-silica.
[0058] Preparation Example 2
[0059] The preparation method of modified maltodextrin A comprises the following steps:
[0060] (1) 0.1 mol of maltodextrin, 0.4 mol of glutaric acid, and 300 ml of water were added to a reaction kettle, mixed and dissolved, and then 0.15 mol of sodium hypophosphite was added, stirred for 20 min, and dried at 80° C. for 6 h to obtain a mixture;
[0061] (2) pouring the mixture obtained in step (1) into a reaction kettle, heating to 150° C., and reacting for 30 min to obtain an intermediate product;
[0062] (3) The intermediate product obtained in step (2) and 200 ml of water were mixed and dissolved, and then 800 ml of anhydrous ethanol was added, the precipitate was filtered, and washed with anhydrous ethanol twice, and vacuum dried at 50° C. for 2 h to obtain a modified product;
[0063] (4) 0.2 mol of the modified product obtained in step (3), 0.6 mol of 2-acrylamide-2-methylpropanesulfonic acid, and 400 ml of water are added to a reaction kettle, and then 0.05 mol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.05 mol of N-hydroxysuccinimide are added, heated to 70° C., and stirred for reaction for 6 hours to obtain modified maltodextrin A.
[0064] Preparation Example 3
[0065] The preparation method of modified maltodextrin B comprises the following steps:
[0066] (1) 0.4 mol of maltodextrin, 0.6 mol of glutaric acid, and 150 ml of water were added to a reaction kettle, mixed and dissolved, and then 0.08 mol of sodium hypophosphite was added, stirred for 20 min, and dried at 80° C. for 6 h to obtain a mixture;
[0067] (2) pouring the mixture obtained in step (1) into a reaction kettle, heating to 150° C., and reacting for 30 min to obtain an intermediate product;
[0068] (3) The intermediate product obtained in step (2) and 100 ml of water were mixed and dissolved, and then 400 ml of anhydrous ethanol was added, the precipitate was filtered, and washed with anhydrous ethanol twice, and vacuum dried at 50° C. for 2 h to obtain a modified product;
[0069] (4) 0.2 mol of the modified product obtained in step (3), 0.6 mol of 2-acrylamide-2-methylpropanesulfonic acid, and 400 ml of water are added to a reaction kettle, and then 0.05 mol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.05 mol of N-hydroxysuccinimide are added, and the mixture is heated to 70° C. and stirred for reaction for 6 hours to obtain modified maltodextrin B.
[0070] Preparation Example 4
[0071] The preparation method of modified maltodextrin C comprises the following steps:
[0072] (1) 0.1 mol of maltodextrin, 0.4 mol of glutaric acid, and 300 ml of water were added to a reaction kettle, mixed and dissolved, and then 0.15 mol of sodium hypophosphite was added, stirred for 20 min, and dried at 80° C. for 6 h to obtain a mixture;
[0073] (2) pouring the mixture obtained in step (1) into a reaction kettle, heating to 150° C., and reacting for 30 min to obtain an intermediate product;
[0074] (3) The intermediate product obtained in step (2) and 200 ml of water were mixed and dissolved, and then 800 ml of anhydrous ethanol was added, the precipitate was filtered, and washed with anhydrous ethanol twice, and vacuum dried at 50° C. for 2 h to obtain a modified product;
[0075] (4) 0.2 mol of the modified product obtained in step (3), 0.3 mol of 2-acrylamide-2-methylpropanesulfonic acid, and 250 ml of water are added to a reaction kettle, and then 0.04 mol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.04 mol of N-hydroxysuccinimide are added, and the mixture is heated to 70° C. and stirred for reaction for 6 hours to obtain modified maltodextrin C.
[0076] Preparation Example 5
[0077] The preparation method of modified 3-mercaptoalanine A comprises the following steps:
[0078] (1) 1.2 mol of 3-mercaptoalanine and 380 ml of water were mixed and added to a reaction kettle, 15 wt % sodium hydroxide solution was added to adjust the pH to 10, and then 1 mol of (R)-benzyloxymethyl oxirane was added dropwise, heated to 60° C., and stirred for reaction for 2.5 hours;
[0079] (2) After the reaction is completed, 10 wt % hydrochloric acid is added to adjust the pH to 7.5, the mixture is allowed to stand for stratification, the lower layer is taken, and the lower layer is concentrated by rotary evaporation to obtain modified 3-mercaptoalanine A.
[0080] Preparation Example 6
[0081] The preparation method of modified 3-mercaptoalanine B comprises the following steps:
[0082] (1) 1.2 mol of 3-mercaptoalanine and 380 ml of water were mixed and added to a reaction kettle, 15 wt % sodium hydroxide solution was added to adjust the pH to 10, and then 0.8 mol of (R)-benzyloxymethyl oxirane was added dropwise, heated to 60° C., and stirred for reaction for 2.5 hours;
[0083] (2) After the reaction is completed, 10 wt % hydrochloric acid is added to adjust the pH to 7.5, the mixture is allowed to stand for stratification, the lower layer is taken, and the lower layer is concentrated by rotary evaporation to obtain modified 3-mercaptoalanine B.
[0084] Example 1
[0085] A temperature-suppressing self-healing concrete anti-cracking waterproofing agent comprises the following raw materials in parts by weight: 20 parts of modified nano-silicon dioxide, 20 parts of modified maltodextrin A, 7.5 parts of sodium metasilicate, 6 parts of sodium gluconate, 4.5 parts of modified 3-mercaptoalanine A, 4 parts of calcium nitrate, 3 parts of potassium hydroxide, 1.5 parts of organosilicon defoaming agent SDF-043, 1.5 parts of polycarboxylate dispersant LY-600, and 40 parts of water.
[0086] The preparation method of the anti-cracking waterproof agent of this embodiment comprises the following steps:
[0087] 1. Add modified nano-silicon dioxide, modified maltodextrin A, sodium metasilicate, sodium gluconate, modified 3-mercaptoalanine A and water into a reactor, stir for 25 minutes, add calcium nitrate and potassium hydroxide in sequence, heat to 35°C, stir for 7 minutes, cool, and obtain a mixed substance;
[0088] 2. Mix the organosilicon defoamer SDF-043 and the polycarboxylate dispersant LY-600, stir for 8 minutes, add the mixed substance obtained in step 1, heat to 35° C., stir for 25 minutes, and obtain an anti-cracking waterproofing agent.
[0089] Example 2
[0090] A temperature-suppressing self-healing concrete anti-cracking waterproofing agent comprises the following raw materials in parts by weight: 10 parts of modified nano-silicon dioxide, 15 parts of modified maltodextrin A, 5 parts of sodium metasilicate, 4 parts of sodium gluconate, 3 parts of modified 3-mercaptoalanine A, 3 parts of calcium nitrate, 2 parts of potassium hydroxide, 1 part of organosilicon defoaming agent SDF-043, 1 part of polycarboxylate dispersant LY-600, and 30 parts of water.
[0091] The preparation method of the anti-cracking waterproof agent of this embodiment comprises the following steps:
[0092] 1. Add modified nano-silicon dioxide, modified maltodextrin A, sodium metasilicate, sodium gluconate, modified 3-mercaptoalanine A and water into a reactor, stir for 20 minutes, add calcium nitrate and potassium hydroxide in sequence, heat to 30°C, stir for 10 minutes, and cool to obtain a mixed substance;
[0093] 2. Mix the organosilicon defoamer SDF-043 and the polycarboxylate dispersant LY-600, stir for 5 minutes, add the mixed substance obtained in step 1, heat to 30° C., stir for 30 minutes, and obtain an anti-cracking waterproofing agent.
[0094] Example 3
[0095] A temperature-suppressing self-healing concrete anti-cracking waterproofing agent comprises the following raw materials in parts by weight: 30 parts of modified nano-silicon dioxide, 25 parts of modified maltodextrin A, 10 parts of sodium metasilicate, 8 parts of sodium gluconate, 6 parts of modified 3-mercaptoalanine A, 5 parts of calcium nitrate, 4 parts of potassium hydroxide, 32 parts of organosilicon defoaming agent SDF-04, 2 parts of polycarboxylate dispersant LY-600, and 50 parts of water.
[0096] The preparation method of the anti-cracking waterproof agent of this embodiment comprises the following steps:
[0097] 1. Add modified nano-silicon dioxide, modified maltodextrin A, sodium metasilicate, sodium gluconate, modified 3-mercaptoalanine A and water into a reactor, stir for 30 minutes, add calcium nitrate and potassium hydroxide in sequence, heat to 40°C, stir for 5 minutes, and cool to obtain a mixed substance;
[0098] 2. Mix the organosilicon defoamer SDF-043 and the polycarboxylate dispersant LY-600, stir for 10 minutes, add the mixed substance obtained in step 1, heat to 40° C., stir for 20 minutes, and obtain an anti-cracking waterproofing agent.
[0099] Example 4
[0100] A temperature-suppressing self-healing concrete anti-cracking waterproofing agent and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified maltodextrin B is used to replace modified maltodextrin A.
[0101] Example 5
[0102] A temperature-suppressing self-healing concrete anti-cracking waterproofing agent and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified maltodextrin C is used to replace modified maltodextrin A.
[0103] Example 6
[0104] A temperature-suppressing self-healing concrete anti-cracking waterproofing agent and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified 3-mercaptoalanine B is used to replace modified 3-mercaptoalanine A.
[0105] Comparative Example 1
[0106] A temperature-suppressing self-healing concrete anti-cracking waterproofing agent and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of hydrophobic nano-silica is used to replace modified nano-silica.
[0107] Comparative Example 2
[0108] A temperature-suppressing self-healing concrete anti-cracking waterproofing agent and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of commercially available maltodextrin is used to replace modified maltodextrin A.
[0109] Comparative Example 3
[0110] A temperature-suppressing self-healing concrete anti-cracking waterproofing agent and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of 3-mercaptoalanine is used to replace modified 3-mercaptoalanine A.
[0111] Effect evaluation:
[0112] The anti-cracking waterproofing agents prepared in the above Examples 1-6 and Comparative Examples 1-3 were tested and analyzed, and the specific results are shown in Table 1.
[0113] In parts by weight, concrete was prepared according to 1200 parts of PO52.5 cement, 480 parts of water, and 60 parts of an anti-cracking waterproofing agent (prepared in the examples and comparative examples).
[0114] Performance Testing:
[0115] (1) Peak temperature and temperature suppression rate: Refer to standard T_CECS10270-2023 "Concrete temperature suppression and anti-cracking waterproofing agent" to conduct a semi-adiabatic temperature rise test on cement paste.
[0116] (2) Self-healing ability: The curing method is soaking in water, and the curing environment is at a temperature of about 25°C. Test method: Make a fine stone concrete pool with dimensions of 500mm×300mm×300mm in length, width and height, and a pool bottom thickness of 50mm; pre-place a 0.4mm thick galvanized iron sheet with a width of 100mm at the bottom of the pool before forming; remove the iron sheet about 12 hours after forming, soak it in water for curing after 24 hours of pouring, and observe the water flow at the cracks to reflect the self-healing performance through the water flow.
[0117] Table 1
[0118]
[0119]
[0120] It can be seen from the results in Table 1 that the anti-cracking waterproofing agents of Examples 1-3 have good hydrothermal inhibition effects and excellent self-healing properties.
[0121] Compared with Example 1, Example 4 changes the molar ratio of maltodextrin and glutaric acid when preparing modified maltodextrin, so that the active functional groups are reduced, the compatibility is deteriorated, and the temperature inhibition effect is deteriorated.
[0122] Compared with Example 1, Example 5 changes the molar ratio of the modified product and 2-acrylamide-2-methylpropane sulfonic acid when preparing modified maltodextrin, which not only reduces the heat resistance of maltodextrin, making its hydration heat inhibition effect worse, but also affects the self-healing performance of the anti-cracking waterproofing agent.
[0123] In Example 6, compared with Example 1, the molar ratio of 3-mercaptoalanine and (R)-benzyloxymethyl oxirane was changed when preparing modified 3-mercaptoalanine. The reduction of epoxy groups reduced the density of the concrete.
[0124] Compared with Example 1, Comparative Example 1 uses commercially available hydrophobic nano-silica to replace modified nano-silica, which has poor dispersibility and reduced self-healing performance.
[0125] In Comparative Example 2, compared with Example 1, commercially available maltodextrin is used to replace modified maltodextrin A. The heat resistance of maltodextrin is deteriorated, which makes the hydration heat inhibition effect worse and also affects the self-healing performance.
[0126] Compared with Example 1, in Comparative Example 3, 3-mercaptoalanine was used to replace the modified 3-mercaptoalanine A, resulting in partial inactivation and reduced self-healing performance.
[0127] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.
Claims
1. A temperature-suppressing self-healing concrete anti-cracking waterproofing agent, characterized in that: The anti-cracking waterproof agent comprises the following raw materials by weight: 10-30 parts of modified nano-silicon dioxide, 15-25 parts of modified maltodextrin, 5-10 parts of sodium metasilicate, 4-8 parts of sodium gluconate, 3-6 parts of modified 3-mercaptoalanine, 3-5 parts of calcium nitrate, 2-4 parts of potassium hydroxide, 1-2 parts of defoaming agent, 1-2 parts of dispersant and 30-50 parts of water.
2. A temperature-suppressing self-healing concrete anti-cracking waterproofing agent according to claim 1, characterized in that: The modified nano silicon dioxide is prepared by modifying the nano silicon dioxide with an unsaturated silane coupling agent.
3. The temperature-suppressing self-healing concrete anti-cracking waterproofing agent according to claim 1, characterized in that: The preparation method of the modified maltodextrin comprises the following steps: (1) adding maltodextrin, glutaric acid and water into a reaction kettle, mixing and dissolving, then adding a catalyst, stirring, and drying to obtain a mixture; (2) pouring the mixture obtained in step (1) into a reaction kettle, heating to 120-180° C., and reacting for 15-40 minutes to obtain an intermediate product; (3) dissolving the intermediate product obtained in step (2) in water, then adding anhydrous ethanol, filtering the precipitate, washing, and drying to obtain a modified product; (4) Add the modified product obtained in step (3), 2-acrylamide-2-methylpropanesulfonic acid, and water into a reaction kettle, then add a carbodiimide condensing agent and an activator, heat to 60-80° C., and stir the reaction for 6-8 hours to obtain modified maltodextrin.
4. A temperature-suppressing self-healing concrete anti-cracking waterproofing agent according to claim 3, characterized in that: The molar ratio of maltodextrin to glutaric acid in step (1) is 1:(2-6).
5. The temperature-suppressing self-healing concrete anti-cracking waterproofing agent according to claim 3, characterized in that: The molar ratio of the modified product to 2-acrylamide-2-methylpropanesulfonic acid in step (4) is 1:(2-4).
6. The temperature-suppressing self-healing concrete anti-cracking waterproofing agent according to claim 1, characterized in that: The preparation method of the modified 3-mercaptoalanine comprises the following steps: S1. Mix 3-mercaptoalanine and water and add them to a reactor, add sodium hydroxide to adjust the pH to alkaline, then add (R)-benzyloxymethyl oxirane dropwise, heat to 50-60°C, and stir to react for 2-3h; S2. After the reaction is completed, hydrochloric acid is added to adjust the pH to neutral, the mixture is allowed to stand for stratification, the lower layer is taken, and concentrated by rotary evaporation to obtain modified 3-mercaptoalanine.
7. A temperature-suppressing self-healing concrete anti-cracking waterproofing agent according to claim 6, characterized in that: The molar ratio of the 3-mercaptoalanine to the (R)-benzyloxymethyl oxirane is (1.1-1.3):
1.
8. The temperature-suppressing self-healing concrete anti-cracking waterproofing agent according to claim 1, characterized in that: The dispersant is a polycarboxylate dispersant.
9. The temperature-suppressing self-healing concrete anti-cracking waterproofing agent according to claim 1, characterized in that: The defoamer is an organosilicon defoamer.
10. A method for preparing the temperature-suppressing self-healing concrete anti-cracking waterproofing agent according to any one of claims 1 to 9, characterized in that: The following steps are included:
1. Add modified nano-silicon dioxide, modified maltodextrin, sodium metasilicate, sodium gluconate, modified 3-mercaptoalanine and water into a reaction kettle, stir for 20-30 minutes, add calcium nitrate and potassium hydroxide in sequence, heat to 30-40°C, stir for 5-10 minutes, cool to obtain a mixed substance; 2. Mix the defoamer and dispersant, stir for 5-10 minutes, add the mixed substance obtained in step 1, heat to 30-40° C., stir for 20-30 minutes, and obtain the anti-cracking waterproofing agent.
Citation Information
Cited By
Modified organic silicon waterproof agent as well as preparation method and application thereof
CN120424580A