Green anti-cracking premixed concrete and preparation method thereof

By using ammonium polyphosphate modified wheat straw fibers and self-repair microcapsules in concrete, crack problems during concrete solidification are solved, high-performance and sustainable crack resistance is achieved, structural life is extended and maintenance is reduced cost.

CN118978365APending Publication Date: 2024-11-19WUHAN ZHONGYANGMING BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411030855.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Concrete is prone to irregular or penetrating shrinkage cracks during the condensation process, resulting in waste of resources and reduced structural strength, and the prior art is difficult to effectively solve this problem.

Method used

Adopt green crack-resistant ready-mixed concrete formula, including silicate cement, ultrafine fly ash, slag powder, river sand, gravel, polycarboxylic acid high-efficiency water reducing agent, waste concrete aggregate, ammonium polyphosphate modified wheat straw fiber and self-healing microcapsules, through carefully designed raw material ratios, improve compressive strength and crack resistance, and realize self-repair of concrete through self-healing microcapsules.

Benefits of technology

It achieves a comprehensive balance of environmental protection, high performance, economy and sustainability, improves the compressive strength and crack resistance of concrete, extends the structure life, reduces construction waste, and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004969885060000061
    Figure BDA0004969885060000061
  • Figure BDA0004969885060000071
    Figure BDA0004969885060000071
  • Figure BDA0004969885060000072
    Figure BDA0004969885060000072
Patent Text Reader

Abstract

The invention relates to the technical field of concrete, and particularly discloses green anti-cracking premixed concrete and a preparation method thereof. The green anti-cracking premixed concrete is prepared from the following raw materials in parts by weight: Portland cement, superfine fly ash, slag powder, river sand, broken stone, a polycarboxylic acid superplasticizer, waste concrete aggregate, ammonium polyphosphate modified wheat straw fibers, self-repairing microcapsules and water. The preparation method of the green anti-cracking premixed concrete comprises the following steps: S1, mixing and stirring the ammonium polyphosphate modified wheat straw fibers, the water and the self-repairing microcapsules to obtain a mixture A; s2, adding Portland cement, superfine fly ash, river sand, gravel, a polycarboxylic acid superplasticizer, waste concrete aggregate and slag powder into the mixture A, and stirring to obtain the green anti-cracking premixed concrete. The prepared green anti-cracking premixed concrete is excellent in anti-cracking performance, non-renewable mine resources are utilized, and the green anti-cracking premixed concrete is green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of concrete technology, and in particular to a green, crack-resistant ready-mixed concrete and a preparation method thereof. Background Art

[0002] Concrete refers to an engineering composite material in which aggregates are bonded together by gel materials. It is a non-homogeneous porous material made by mixing cement as gel material, sand and gravel as aggregates with water in a certain proportion, stirring evenly, compacting, curing and hardening.

[0003] Concrete is the most commonly used in construction projects. With the promotion of concrete materials, a lot of waste concrete and bricks are produced. They contain a lot of non-renewable mining resources, and direct dumping causes waste of resources.

[0004] In addition, after the concrete is poured, many quality problems often occur, such as irregular or through shrinkage cracks in the concrete during the setting process. There are many reasons for concrete cracking: First, before the concrete sets, cement is a hydraulic material with shrinkage. In the early stage of hardening, it will shrink and crack due to rapid surface water loss; second, after the concrete is mixed, some alkali ions will be produced. These ions will react chemically with certain active aggregates and absorb water from the surrounding environment to increase in volume, causing the concrete to expand and crack, and produce alkali-aggregate reaction cracks; third, concrete is a non-homogeneous porous material with many pores and capillaries inside, which causes external moisture to enter the concrete, weakening the overall strength of the concrete and causing cracks. Summary of the invention

[0005] In order to solve at least one of the above technical problems, the present application provides a green crack-resistant ready-mixed concrete and a preparation method thereof.

[0006] On the one hand, the present application provides a green crack-resistant ready-mixed concrete, comprising the following raw materials in parts by weight: 100-120 parts of silicate cement, 35-45 parts of ultrafine fly ash, 30-40 parts of slag powder, 180-210 parts of river sand, 190-220 parts of crushed stone, 3-7 parts of polycarboxylic acid high-efficiency water reducer, 40-65 parts of waste concrete aggregate, 8-14 parts of ammonium polyphosphate modified wheat straw fiber, 12-21 parts of self-healing microcapsules, and 60-72 parts of water.

[0007] By adopting the above technical scheme, the present application achieves a comprehensive balance of environmental protection, high performance, economy and sustainability through a carefully designed raw material ratio, improves the compressive strength and crack resistance of concrete, and realizes the self-repair efficiency of concrete after cracking.

[0008] Waste concrete aggregates are used as recycled aggregates to achieve resource recycling, reduce construction waste, be environmentally friendly, and do not affect the basic properties of concrete; the addition of wheat straw fiber can effectively reduce the plastic shrinkage and drying shrinkage of concrete, thereby reducing the risk of cracking. Wheat straw fiber is modified with ammonium polyphosphate to obtain ammonium polyphosphate modified wheat straw fiber, which has better dispersibility and compatibility with the concrete matrix, can effectively improve the bonding force between fiber and concrete, enhance the crack resistance of concrete, and resist the generation of cracks during long-term use; the self-healing microcapsules containing repair agents will rupture when cracks occur inside the concrete, release the repair agent, and automatically repair concrete microcracks, thereby extending the life of the structure and improving durability.

[0009] The preparation method of the ammonium polyphosphate modified wheat straw fiber comprises the following steps: A1, respectively dissolving ammonium polyphosphate and pure acrylic emulsion in water for dilution to obtain an ammonium polyphosphate aqueous solution and a pure acrylic emulsion aqueous solution; A2. Spray the ammonium polyphosphate aqueous solution obtained in step A1 on the surface of the wheat straw fiber, spray the pure acrylic emulsion aqueous solution obtained in step A1 after drying, and perform drying treatment after drying to obtain the ammonium polyphosphate modified wheat straw fiber.

[0010] Optionally, the weight ratio of the ammonium polyphosphate, pure acrylic emulsion and wheat straw fiber is (55-65):100:(38-45).

[0011] Optionally, the dilution ratio of the ammonium polyphosphate is 2:5, and the dilution ratio of the pure acrylic emulsion is 1:1.

[0012] Optionally, the method for preparing the self-repairing microcapsules comprises the following steps: B1, adding gum arabic to water, mixing, heating to dissolve, then adding montmorillonite, stirring and mixing, and ultrasonically dispersing for 15-20 minutes to obtain a mixture I; diphenylmethane diisocyanate and hexamethylene diisocyanate are stirred and mixed to obtain a mixture II; B2, mixing mixture I and mixture II and stirring for 40-45 minutes, and emulsifying to obtain an emulsion; B3. Add a 0.8% triethylenetetramine solution dropwise into the emulsion, heat and react for 1.5-2 hours, filter, wash, and dry at 45-50° C. for 10-12 hours to obtain the self-repairing microcapsules.

[0013] Through the above technical solution, the present application uses gum arabic and montmorillonite as capsule wall materials, diphenylmethane diisocyanate and hexamethylene diisocyanate as repair agents as core materials to prepare self-repairing microcapsules. When concrete is subjected to external forces to produce microcracks, the microcapsules located near the cracks rupture due to stress concentration, releasing the isocyanate repair agent inside. The released isocyanate repair agent comes into contact with the water in the concrete or the moisture in the air, undergoes a polymerization reaction, and generates high molecular substances such as polyurethane to fill the cracks. The self-repair of the concrete structure is achieved, the crack resistance of the concrete is improved, the life of the concrete is increased, and the maintenance cost is reduced.

[0014] Optionally, in step B1, the weight ratio of gum arabic, water and montmorillonite is (2-4):100:(1-2), and the weight ratio of diphenylmethane diisocyanate and hexamethylene diisocyanate is 1:(4-5).

[0015] Optionally, in step B3, the volume ratio of the triethylenetetramine solution to the emulsion is 1:2.

[0016] Optionally, the weight ratio of the ammonium polyphosphate modified wheat straw fiber to the self-healing microcapsule is 1:(1-1.8).

[0017] Optionally, the weight ratio of the ammonium polyphosphate modified wheat straw fiber to the self-healing microcapsule is 1:1.5.

[0018] Optionally, the sum of the weights of the ammonium polyphosphate modified wheat straw fibers and the self-repairing microcapsules accounts for 2.7-4.0% of the total weight of the green anti-cracking ready-mixed concrete raw materials.

[0019] By adopting the above technical scheme, the present application limits the weight ratio of ammonium polyphosphate modified wheat straw fiber and self-healing microcapsules, as well as the weight and proportion of the two in the concrete raw materials, to ensure that the concrete has both good crack resistance and good self-healing ability, and avoids the problem that too little fiber may not be enough to effectively inhibit crack propagation, and too much microcapsules may lead to increased costs and decreased mechanical properties.

[0020] In a second aspect, the present application provides a method for preparing the above-mentioned green crack-resistant ready-mixed concrete, comprising the following steps: S1, mixing ammonium polyphosphate modified wheat straw fiber, water and self-repairing microcapsules to obtain a mixture A; S2. Adding silicate cement, ultrafine fly ash, river sand, crushed stone, polycarboxylic acid high-efficiency water reducing agent, waste concrete aggregate and slag powder into mixture A and stirring to obtain the green anti-cracking ready-mixed concrete.

[0021] By adopting the above technical solution, the preparation method of the present application is simple, the obtained crack-resistant concrete has excellent performance and is suitable for popularization and application.

[0022] In summary, the present invention includes at least one of the following beneficial technical effects: 1. This application achieves a comprehensive balance of environmental protection, high performance, economy and sustainability through a carefully designed raw material ratio, improves the compressive strength and crack resistance of concrete, and achieves the self-repair efficiency of concrete after cracking. Waste concrete aggregate is used as recycled aggregate to achieve resource recycling, reduce construction waste, be environmentally friendly, and do not affect the basic properties of concrete; wheat straw fiber is modified with ammonium polyphosphate to obtain ammonium polyphosphate modified wheat straw fiber, which can effectively improve the bonding force between fiber and concrete, enhance the crack resistance of concrete, and resist the generation of cracks during long-term use; the self-repairing microcapsules containing repair agents rupture when cracks occur inside the concrete, release the repair agent, and automatically repair concrete microcracks, extend the life of the structure, and improve durability.

[0023] 2. This application limits the weight ratio of ammonium polyphosphate modified wheat straw fiber and self-healing microcapsules, as well as the weight and proportion of the two in the concrete raw materials, to ensure that the concrete has both good crack resistance and good self-healing ability, and to avoid problems such as too little fiber may not be enough to effectively inhibit crack propagation, and too much microcapsules may lead to increased costs and decreased mechanical properties.

[0024] 3. The preparation method of the present application is simple, and the crack-resistant concrete obtained has excellent performance and is suitable for popularization and application. DETAILED DESCRIPTION

[0025] The present application is further described in detail below with reference to the embodiments. Specific embodiments

[0026] Preparation Example 1 This preparation example provides an ammonium polyphosphate modified wheat straw fiber, and the preparation method comprises the following steps: A1, respectively dissolving ammonium polyphosphate and pure acrylic emulsion in water for dilution to obtain an ammonium polyphosphate aqueous solution and a pure acrylic emulsion aqueous solution; A2. Spray the ammonium polyphosphate aqueous solution obtained in step A1 on the surface of the wheat straw fiber, spray the pure acrylic emulsion aqueous solution obtained in step A1 after drying, and perform drying treatment after drying to obtain the ammonium polyphosphate modified wheat straw fiber.

[0027] The weight ratio of the ammonium polyphosphate, the pure acrylic emulsion and the wheat straw fiber is 60:100:40.

[0028] The dilution ratio of the ammonium polyphosphate is 2:5, and the dilution ratio of the pure acrylic emulsion is 1:1.

[0029] Preparation Example 2 This preparation example provides a self-repairing microcapsule, and the preparation method comprises the following steps: B1, adding gum arabic to water, mixing, heating to dissolve, then adding montmorillonite, stirring and mixing, and ultrasonically dispersing for 20 minutes to obtain a mixture I; diphenylmethane diisocyanate and hexamethylene diisocyanate were stirred and mixed to obtain a mixture II; B2, mixing mixture I and mixture II and stirring for 45 minutes, and emulsifying to obtain an emulsion; B3. Add a 0.8% triethylenetetramine solution dropwise into the emulsion, heat and react for 2 hours, filter, wash, and dry at 50° C. for 12 hours to obtain the self-repairing microcapsules.

[0030] In the step B1, the weight ratio of gum arabic, water and montmorillonite is 3:100:1.5, and the weight ratio of diphenylmethane diisocyanate and hexamethylene diisocyanate is 1:4.5; in the step B3, the volume ratio of triethylenetetramine solution and emulsion is 1:2.

[0031] Example 1 The present embodiment provides a green anti-cracking ready-mixed concrete, comprising the following raw materials in parts by weight: 100 parts of silicate cement, 35 parts of ultrafine fly ash, 30 parts of slag powder, 180 parts of river sand, 190 parts of crushed stone, 3 parts of polycarboxylic acid high-efficiency water reducing agent, 40 parts of waste concrete aggregate, 10 parts of ammonium polyphosphate modified wheat straw fiber, 15 parts of self-repairing microcapsules, and 60 parts of water.

[0032] The preparation method of green crack-resistant ready-mixed concrete in this embodiment comprises the following steps: S1, mixing the ammonium polyphosphate modified wheat straw fiber prepared in Preparation Example 1, water and the self-repairing microcapsules prepared in Preparation Example 2 to obtain a mixture A; S2. Adding silicate cement, ultrafine fly ash, river sand, crushed stone, polycarboxylic acid high-efficiency water reducing agent, waste concrete aggregate and slag powder into mixture A and stirring to obtain the green anti-cracking ready-mixed concrete.

[0033] Embodiment 2-4 Example 2 The difference between this embodiment and embodiment 1 is that when preparing green crack-resistant ready-mixed concrete, the total weight of ammonium polyphosphate-modified wheat straw fiber and self-repairing microcapsules is 25 parts, and the weight ratio of ammonium polyphosphate-modified wheat straw fiber to self-repairing microcapsules is 1:1.

[0034] Example 3 The difference between this embodiment and embodiment 1 is that when preparing green crack-resistant ready-mixed concrete, the total weight of ammonium polyphosphate-modified wheat straw fiber and self-repairing microcapsules is 25 parts, and the weight ratio of ammonium polyphosphate-modified wheat straw fiber to self-repairing microcapsules is 1:1.2.

[0035] Example 4 The difference between this embodiment and embodiment 1 is that when preparing green crack-resistant ready-mixed concrete, the total weight of ammonium polyphosphate-modified wheat straw fiber and self-repairing microcapsules is 25 parts, and the weight ratio of ammonium polyphosphate-modified wheat straw fiber to self-repairing microcapsules is 1:1.8.

[0036] Comparative Examples 1-3 Comparative Example 1 The difference between this comparative example and Example 1 is that no self-repairing microcapsules are added when preparing the green crack-resistant ready-mixed concrete.

[0037] Comparative Example 2 The difference between this comparative example and Example 1 is that ammonium polyphosphate modified wheat straw fiber is not added when preparing the green crack-resistant ready-mixed concrete.

[0038] Comparative Example 3 The difference between this comparative example and Example 1 is that ammonium polyphosphate-modified wheat straw fiber and self-repairing microcapsules are not added when preparing the green crack-resistant ready-mixed concrete.

[0039] Experimental testing: Compressive strength test: According to GB / T 50081-2002, the compressive strength test of the green crack-resistant ready-mixed concrete specimens prepared in the examples and comparative examples of the present application was carried out, and the 28d compressive strength F1 of each specimen was measured; Crack resistance test: According to JGJ / T 193-2009, the crack resistance test was carried out on the specimens of the green crack-resistant ready-mixed concrete prepared in the examples and comparative examples of the present application; Self-repair ability test: the green crack resistant ready-mixed concrete test blocks were pre-compressed and damaged (the pre-compression value was 60% of the compressive strength), and then the compressive strength F2 of each test block after pre-compression and damage was tested. The damaged test blocks were then steam-oxidized at 50°C and cured for 3 days. The compressive strength F3 of the green crack resistant ready-mixed concrete test blocks after 3 days of repair was tested, and the compressive strength repair rate of each green crack resistant ready-mixed concrete test block was calculated: W1(%) = (F3-F2) / F2×100%, which is used to characterize the self-repair ability of green crack resistant ready-mixed concrete.

[0040] The experimental test results of Examples 1-4 and Comparative Examples 1-3 are shown in Table 1.

[0041] Table 1 Experimental test results of Examples 1-4 and Comparative Examples 1-3 Example <![CDATA[F1(MPa)]]> <![CDATA[W1(%)]]> Crack resistance grade Example 1 83.5 18.6 LV Example 2 76.1 14.8 L-IV Example 3 79.7 16.2 L-IV Example 4 80.6 17.5 L-IV Comparative Example 1 69.8 0 L-III Comparative Example 2 64.4 12.1 L-III Comparative Example 3 55.1 0 L-II Result analysis: The difference between Examples 2-4 and Example 1 is that when preparing green anti-cracking ready-mixed concrete, the total weight of ammonium polyphosphate modified wheat straw fiber and self-repairing microcapsules is 25 parts, and the weight ratio of ammonium polyphosphate modified wheat straw fiber and self-repairing microcapsules is different. Combined with the experimental test results in Table 1, it can be seen that when the weight ratio of ammonium polyphosphate modified wheat straw fiber and self-repairing microcapsules is 1:1.5, the green anti-cracking ready-mixed concrete obtained has high compressive strength, good crack resistance, and good self-repairing ability. The difference between Comparative Example 1 and Example 1 is that when preparing green anti-cracking ready-mixed concrete, no self-repairing microcapsules are added. The difference between Comparative Example 2 and Example 1 is that when preparing green anti-cracking ready-mixed concrete, no ammonium polyphosphate modified wheat straw fiber is added. The difference between Comparative Example 3 and Example 1 is that when preparing green anti-cracking ready-mixed concrete, no ammonium polyphosphate modified wheat straw fiber and self-repairing microcapsules are added. Combined with the experimental test results in Table 1, it can be seen that when preparing green crack-resistant ready-mixed concrete, the compound use of ammonium polyphosphate modified wheat straw fiber and self-repairing microcapsules can better improve the comprehensive performance of the green crack-resistant ready-mixed concrete.

[0042] Embodiment 5-6 Example 5 The difference between Example 5-6 and Example 1 is that the weight percentages of some components are changed when preparing the green crack-resistant ready-mixed concrete. See Table 2 for the differences.

[0043] Table 2 Differences between Examples 5-6 and Example 3 Ingredients (parts by weight) Example 3 Example 5 Example 6 Portland cement 100 115 120 Ultrafine fly ash 35 40 45 Slag powder 30 38 40 river sand 180 200 210 gravel 190 205 220 Polycarboxylate high efficiency water reducer 3 5 7 Waste concrete aggregate 40 52 65 Ammonium polyphosphate modified wheat straw fiber 10 10 10 Self-healing microcapsules 15 15 15 water 60 64 72 The experimental test results of Examples 5-6 are shown in Table 3.

[0044] Table 3 Experimental test results of Examples 5-6 Result analysis: The difference between Example 5-6 and Example 1 is that when preparing green crack-resistant premixed concrete, the weight proportions of some components are different. Combined with the experimental test results in Table 3, it can be seen that when preparing green crack-resistant premixed concrete, the comprehensive performance of the green crack-resistant premixed concrete prepared in Example 5 is better.

[0045] Embodiment 7-9 The difference between Example 7-9 and Example 5 is that when preparing green anti-cracking ready-mixed concrete, on the premise that the weight ratio of ammonium polyphosphate modified wheat straw fiber and self-repairing microcapsules is 1:1.5, the total weight of ammonium polyphosphate modified wheat straw fiber and self-repairing microcapsules in the total weight of green anti-cracking ready-mixed concrete raw materials is changed, and the optimal weight ratio is selected.

[0046] In Example 5, the total weight of ammonium polyphosphate modified wheat straw fiber and self-repairing microcapsules is 25 parts, and the total weight of green anti-cracking ready-mixed concrete raw materials is 744 parts.

[0047] Therefore, it is not difficult to conclude that in Example 5, the proportion of ammonium polyphosphate modified wheat straw fiber (called variable 1) and self-healing microcapsules (called variable 2) in the total weight of green anti-cracking ready-mixed concrete raw materials (called matrix) is 3.36%.

[0048] The differences between Examples 7-9 and Example 5 are shown in Table 4.

[0049] Proportion = (variable 1 + variable 2) / total weight of matrix * 100%.

[0050] Table 4 Differences between Examples 7-9 and Example 5 The experimental test results of Examples 7-9 are shown in Table 5.

[0051] Table 5 Experimental test results of Examples 7-9 Example <![CDATA[F1(MPa)]]> <![CDATA[W1(%)]]> Crack resistance grade Example 5 85.1 19.8 LV Example 7 82.8 18.5 LV Example 8 84.1 19.2 LV Example 9 80.9 17.8 L-IV Results analysis: The difference between Examples 7-9 and Example 5 is that when preparing green crack-resistant ready-mixed concrete, when the proportion of ammonium polyphosphate modified wheat straw fiber (referred to as variable 1) and self-repairing microcapsules (referred to as variable 2) in the total weight of the green crack-resistant ready-mixed concrete raw materials (referred to as the matrix) is between (2.7-4.0)%, the comprehensive performance of the green crack-resistant ready-mixed concrete is better. When the proportion of ammonium polyphosphate modified wheat straw fiber (referred to as variable 1) and self-repairing microcapsules (referred to as variable 2) in the green crack-resistant ready-mixed concrete (referred to as the matrix) is 3.36%, the comprehensive performance of the green crack-resistant ready-mixed concrete is better.

[0052] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A green crack-resistant ready-mixed concrete, characterized in that: The invention comprises the following raw materials in parts by weight: 100-120 parts of silicate cement, 35-45 parts of ultrafine fly ash, 30-40 parts of slag powder, 180-210 parts of river sand, 190-220 parts of crushed stone, 3-7 parts of polycarboxylic acid high-efficiency water reducing agent, 40-65 parts of waste concrete aggregate, 8-14 parts of ammonium polyphosphate modified wheat straw fiber, 12-21 parts of self-repairing microcapsules and 60-72 parts of water.

2. The green crack-resistant ready-mixed concrete according to claim 1, characterized in that: The preparation method of the ammonium polyphosphate modified wheat straw fiber comprises the following steps: A1, respectively dissolving ammonium polyphosphate and pure acrylic emulsion in water for dilution to obtain an ammonium polyphosphate aqueous solution and a pure acrylic emulsion aqueous solution; A2. Spray the ammonium polyphosphate aqueous solution obtained in step A1 on the surface of the wheat straw fiber, spray the pure acrylic emulsion aqueous solution obtained in step A1 after drying, and perform drying treatment after drying to obtain the ammonium polyphosphate modified wheat straw fiber.

3. The green crack-resistant ready-mixed concrete according to claim 2, characterized in that: The weight ratio of the ammonium polyphosphate, pure acrylic emulsion and wheat straw fiber is (55-65):100:(38-45).

4. The green crack-resistant ready-mixed concrete according to claim 2, characterized in that: The dilution ratio of the ammonium polyphosphate is 2:5, and the dilution ratio of the pure acrylic emulsion is 1:

1.

5. The green crack-resistant ready-mixed concrete according to claim 1, characterized in that: The method for preparing the self-repairing microcapsules comprises the following steps: B1, adding gum arabic to water, mixing, heating to dissolve, then adding montmorillonite, stirring and mixing, and ultrasonically dispersing for 15-20 minutes to obtain a mixture I; diphenylmethane diisocyanate and hexamethylene diisocyanate are stirred and mixed to obtain a mixture II; B2, mixing mixture I and mixture II and stirring for 40-45 minutes, and emulsifying to obtain an emulsion; B3. Add a 0.8% triethylenetetramine solution dropwise into the emulsion, heat and react for 1.5-2 hours, filter, wash, and dry at 45-50° C. for 10-12 hours to obtain the self-healing microcapsules.

6. The green crack-resistant ready-mixed concrete according to claim 5, characterized in that: In the step B1, the weight ratio of gum arabic, water and montmorillonite is (2-4):100:(1-2), and the weight ratio of diphenylmethane diisocyanate and hexamethylene diisocyanate is 1:(4-5).

7. The green crack-resistant ready-mixed concrete according to claim 1, characterized in that: The weight ratio of the ammonium polyphosphate modified wheat straw fiber to the self-repairing microcapsule is 1:(1-1.8).

8. The green crack-resistant ready-mixed concrete according to claim 1, characterized in that: The weight ratio of the ammonium polyphosphate modified wheat straw fiber to the self-repairing microcapsule is 1:1.

5.

9. The green crack-resistant ready-mixed concrete according to claim 1, characterized in that: The total weight of the ammonium polyphosphate modified wheat straw fiber and the self-repairing microcapsules accounts for 2.7-4.0% of the total weight of the green anti-cracking ready-mixed concrete raw materials.

10. A method for preparing the green crack-resistant ready-mixed concrete according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1, mixing ammonium polyphosphate modified wheat straw fiber, water and self-repairing microcapsules to obtain a mixture A; S2. Adding silicate cement, ultrafine fly ash, river sand, crushed stone, polycarboxylic acid high-efficiency water reducing agent, waste concrete aggregate and slag powder into mixture A and stirring to obtain the green anti-cracking ready-mixed concrete.