Hole slag sand powder high-toughness cement-based material for jetting construction of surrounding rock large-deformation tunnel

By using a combination of hard cave slag sand powder and a variety of energy-consuming components, a high toughness cement-based material suitable for large deformation tunnels in surrounding rocks was prepared, which solved the problems of high cost of existing materials and low resource utilization. It achieves the improvement of high toughness and durability of the material, and is suitable for complex stress fields and high temperature difference environments.

CN118978367AActive Publication Date: 2024-11-19RAILWAY CONSTR RES INST OF CHINA ACAD OF RAILWAY SCI CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411047241.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing high-toughness cement-based materials have high cost, complex composition and difficult to control in the construction of large-deformed surrounding rock tunnels under extremely complex stress fields. Moreover, traditional materials cannot effectively utilize hard cave slag resources, resulting in resource waste and environmental pollution.

Method used

Hard cave slag sand powder is used as aggregate, combined with microscopic and mesoscopic energy-consuming components, and materials such as calcium carbonate whiskers, calcium sulfate whiskers, polyvinyl alcohol fibers, basalt fibers and alkali-resistant glass fibers are used to combine with alkali-free speed A high toughness cement-based material suitable for large deformation tunnel jet construction of surrounding rocks is prepared by a defensive polycarboxylic acid water reducing agent.

Benefits of technology

It achieves high static ductility, good durability and low comprehensive cost of the material. It can effectively utilize waste cave slag resources and improve the support capacity of large deformation tunnels in surrounding rocks. It is suitable for complex stress fields and high temperature differences.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004973818480000081
    Figure BDA0004973818480000081
  • Figure BDA0004973818480000091
    Figure BDA0004973818480000091
Patent Text Reader

Abstract

The invention discloses a hole slag sand powder high-toughness cement-based material for jetting construction of a surrounding rock large-deformation tunnel and a preparation method thereof, and belongs to the field of building materials, the hole slag sand powder high-toughness cement-based material comprises the following raw materials: 600-1000 parts of Portland cement, 300-600 parts of hole slag sand powder, 50-100 parts of a microscopic energy consumption component, 20-60 parts of a microcosmic energy consumption component, 60-100 parts of an accelerator, 2-5 parts of a working performance regulating material and 350-500 parts of water. According to the prepared high-toughness cement-based material, the hard rock waste hole slag sand powder is adopted to replace superfine quartz sand in a traditional material, the microcosmic energy consumption component and the microcosmic energy consumption component are adopted as toughening and energy absorbing components, and the obtained high-toughness cement-based material is high in static ductility, good in durability, low in comprehensive cost and suitable for large-scale production. Meanwhile, a recycling mode is provided for the waste hole slag, and the method has wide application prospects in railway and highway extremely complex stress field surrounding rock large-deformation tunnels, large-temperature-difference circulating bridge pier outer protection layers and bridge deck plate paving.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a high-toughness cement-based material of slag sand powder used for jetting construction of tunnels with large surrounding rock deformation. Background Art

[0002] As my country's railway, highway and other infrastructure construction is advancing to the central and western regions and the plateau and mountainous areas, tunnel disaster control under high geostress has become a key technical problem affecting the quality of the project and the progress of the construction. The surrounding rock of the hard rock section under high geostress stores a large amount of elastic energy. The role of the structural surface is significantly reduced when the rock mass is excavated and destroyed, showing phenomena such as spalling, buckling, plate cracking, and rock burst, which cause engineering accidents such as tunnel collapse, TBM jamming, and steel arch yield fracture, which also pose a serious threat to the safe service of the tunnel. High geostress hard rock can be ensured to be stable by stress release methods such as drilling and pre-blasting, and can also be reinforced by support methods with energy absorption capacity. For tunnels with large deformation of the surrounding rock, controlling the deformation of the surrounding rock within the allowable range, adopting the "yield pressure support" method, and using the high toughness and active deformation of the tunnel concrete to release the surrounding rock energy under geostress are effective ways to solve the large deformation of the tunnel surrounding rock under high geostress. Steel fiber shotcrete and high-performance polypropylene fiber reinforced shotcrete have become widely used primary support materials due to their high strength grade and high toughness and energy absorption. However, for extremely complex stress fields with frequent crustal activities, tunnel surrounding rock deformation is greater under high ground stress, and high-toughness cement-based materials are urgently needed to replace traditional shotcrete as the primary support material for the tunnel.

[0003] Traditional high-toughness cement-based materials use cement, admixtures, fine aggregates, fibers and additives as raw materials. Their ultimate tensile strain is not less than 0.5%, and they show multi-crack cracking characteristics under tensile stress. They are also called engineering cement-based materials (ECC) or strain-hardening cement-based materials (SHCC). Traditional ECC relies on clean ultrafine quartz sand (maximum particle size less than 0.3mm) as aggregate, and polyethylene fiber (PE) or polyvinyl alcohol fiber (PVA) as toughening components, which has high requirements for raw materials. In the central and western regions and the rugged mountainous areas of the plateau, it is difficult to purchase and transport ultrafine quartz sand and fly ash, which makes the cost of high-toughness cement-based materials prepared by conventional technology high, and it is difficult to meet the needs of large-scale use of tunnels with extremely complex stress fields and large deformation of surrounding rocks.

[0004] Application CN 115477518 A discloses a sprayable ultra-high toughness cement-based composite material and its preparation method and application. It uses cement, fly ash, calcined clay, limestone and calcined magnesium oxide as cementitious materials and quartz sand as aggregate. The material sources are diverse and it is difficult to apply under extremely complex stress fields.

[0005] Application CN 110981404 A discloses an ultra-high ductility cement-based material for repair and reinforcement, which proposes an ultra-high ductility cement-based material ratio, in which nanoparticles, microcapsules, PVA fibers or PE fibers are used. The material components are relatively complex, the overall cost is high, and the adaptability to on-site spraying construction is insufficient.

[0006] Application CN 114634338 A discloses a high-ductility cement-based composite material of desert aeolian sand and a preparation method thereof. It discloses a method for preparing a high-ductility material using aeolian sand, which makes full use of the aeolian sand resources in the desert. However, its molding method is vibration molding, which is not suitable for the needs of tunnel jetting construction.

[0007] Application CN 115448647 A discloses a high-ductility recycled powder geopolymer-based reinforcement and repair material and a preparation method thereof. The geopolymer is used as a repair and reinforcement material to achieve secondary utilization of recycled sand powder. However, the geopolymer material has a too fast setting time and has high maintenance requirements. It is prone to cracking during on-site spraying construction and may have insufficient durability.

[0008] It can be seen from the above that although there are many high-toughness cement-based materials, most of them are complex in composition, high in cost, and difficult to control in construction performance. There is still a lack of high-toughness and high-durability cement-based materials suitable for jetting construction of tunnels with large deformation in extremely complex stress fields. On the other hand, according to the provisions of "Machinery Sand for Railway Concrete" (Q / CR 865), hard rock slag (the uniaxial saturated compressive strength of the parent rock is greater than 30MPa but less than 60MPa) cannot be used to produce ballast, crushed stone for concrete and machine-made sand. The disposal of hard rock slag not only occupies a large amount of land resources and damages the ecological environment, but also easily induces secondary disasters such as landslides.

[0009] In view of the lack of high-quality raw materials in dangerous areas, hard rock tunnel slag is used to produce slag sand powder, thereby preparing high-toughness cement-based materials, realizing "take from the tunnel, use in the tunnel". This is not only a beneficial method to solve the resource utilization of waste slag, but also has important significance for improving the support capacity of tunnels with large deformation of surrounding rocks.

[0010] Therefore, it is a technical problem that technicians in this field need to solve urgently to provide a high-toughness cement-based material made of hard rock slag as raw material for jet construction of tunnels with large deformation of surrounding rocks. Summary of the invention

[0011] In view of this, the present invention provides a high-toughness cement-based material of slag sand powder for jetting construction of tunnels with large surrounding rock deformation.

[0012] In order to achieve the above object, the present invention adopts the following technical solution:

[0013] A high-toughness cement-based material of slag sand powder for jetting construction of tunnels with large deformation of surrounding rocks, comprising the following raw materials in parts by weight: 600-1000 parts of silicate cement, 300-600 parts of slag sand powder, 50-100 parts of microscopic energy-consuming components, 20-60 parts of mesoscopic energy-consuming components, 60-100 parts of accelerator, 2-5 parts of working performance regulating materials and 350-500 parts of water.

[0014] Furthermore, the parent rock of the slag sand powder is hard rock, and the uniaxial saturated compressive strength of the hard rock is 30-60MPa.

[0015] Furthermore, the particle size of the slag sand powder is less than 2.36 mm, the crushing index is less than 10%, and the MB value is less than 1.0 g / kg.

[0016] The beneficial effect of adopting the above-mentioned further scheme is that the present invention utilizes hard rock slag sand powder to replace the ultrafine quartz sand commonly used in traditional high-toughness cement-based materials, does not use mineral admixtures such as fly ash, and has a simple raw material composition. At the same time, it solves the problem that the saturated compressive strength of hard rock is insufficient and cannot be used as coarse and fine aggregates for concrete, thereby improving the resource utilization rate of waste slag. The prepared high-toughness cement-based material for spraying is used for the spraying construction of tunnels with large deformation of surrounding rocks, realizing the "take from the tunnel, use in the tunnel" of tunnel slag.

[0017] Furthermore, the microscopic energy-consuming component is calcium carbonate whisker and / or calcium sulfate whisker;

[0018] The beneficial effect of adopting the above further scheme is that the microscopic energy-consuming component of the present invention is a mixture of calcium carbonate whiskers and calcium sulfate whiskers, and the particle size is relatively small. It can play a certain role as a crystal nucleus in the cement hydration process, thereby improving the early strength of the cement-based material. At the same time, the microscopic energy-consuming component can fill the voids in the cement-based material, increase the density of the cement-based material, and improve the durability of the material.

[0019] The whisker length in the micro energy-consuming component is 30-50 μm, and the aspect ratio is 20-40.

[0020] Furthermore, the microscopic energy dissipation component is a mixture of any two or three of polyvinyl alcohol fiber, basalt fiber and alkali-resistant glass fiber.

[0021] The beneficial effect of adopting the above further scheme is that the micro-energy-consuming component used in the present invention is a mixture of two or three of PVA, BF, and GF, and the low tensile strength and high elongation at break of PVA fibers and the high tensile strength and medium elongation at break of BF and GF fibers are utilized to achieve the synergy of tensile strength and elongation at break of the micro-energy-consuming components, thereby enhancing the toughness of cement-based materials.

[0022] Furthermore, the fiber monofilament used in the microscopic energy-consuming component has a length of 8-30 mm, an aspect ratio of 200-2000, and an elongation at break greater than 3%.

[0023] Preferably, the microscopic energy dissipation component is obtained by mixing polyvinyl alcohol fiber, basalt fiber and alkali-resistant glass fiber in a mass ratio of 20%-40%: 20%-80%: 20%-80%.

[0024] The beneficial effect of adopting the above-mentioned further scheme is that: the present invention uses nano whiskers and mixed fibers as energy-absorbing components, and the initial branch of the tunnel is deformed under the action of high ground stress. First, relying on the reinforcement and crack-blocking effect of the microscopic energy-absorbing components, the generation of microcracks in the cement-based material is reduced. As the deformation increases, relying on the bridging effect of the mesoscopic energy-absorbing components, multi-crack cracking of the cement-based material is achieved, and the initial crack strength and ultimate strain of the cement-based material are improved, thereby playing a toughening and strengthening role at both the meso and micro scales.

[0025] Furthermore, the working performance regulating material is a viscosity-reducing polycarboxylic acid water-reducing agent with a water-reducing rate greater than 30%.

[0026] Furthermore, the quick-setting agent is an alkali-free quick-setting agent, and the final setting time of the net slurry of the alkali-free quick-setting agent is less than 5 minutes, and the 90d compressive strength retention rate is greater than 105%.

[0027] The present invention also provides a method for preparing the above-mentioned high-toughness cement-based material of slag sand powder for jetting construction of tunnels with large surrounding rock deformation, comprising the following steps:

[0028] (1) Add silicate cement, slag sand powder and micro energy-consuming components into a mixer and dry mix for 2-3 minutes;

[0029] (2) adding working performance regulating materials and 90% of water;

[0030] (3) Add the microscopic energy-consuming components and the remaining water and stir rapidly for 3-5 minutes;

[0031] (4) Add an accelerator to obtain a high-toughness cement-based material for tunnel slag sand powder spraying construction with large surrounding rock deformation.

[0032] The beneficial effects of the present invention are as follows: the high-toughness cement-based material prepared by the present invention adopts hard rock waste cave slag sand powder to replace the ultrafine quartz sand used in traditional high-toughness cement-based materials, and adopts mesoscopic energy-consuming components + microscopic energy-consuming components as toughening and energy-absorbing components. The prepared high-toughness cement-based material has the advantages of high static ductility, good durability and low comprehensive cost, and provides a way to reuse waste cave slag. It has broad application prospects in railway and highway extremely complex stress field surrounding rock large deformation tunnels, large temperature difference cycle bridge pier outer protective layer, and bridge deck paving. DETAILED DESCRIPTION

[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] High-toughness cement-based materials for tunnel spraying construction with large deformation of surrounding rock, raw materials and 1m 3 The dosage of high toughness material is as follows:

[0036] Portland cement: Beijing Jinyu P·O 42.5 cement that meets the requirements of GB / 175-2007, with a dosage of 800kg;

[0037] Cave slag sand powder: The parent rock uniaxial saturated compressive strength is 49.7MPa dolomite, the maximum particle size of the sand powder is 2.36mm, the crushing index is 8.5%, the MB value is 0.8g / kg, and the dosage is 500kg;

[0038] Working performance control material: PCEA-1 viscosity-reducing polycarboxylic acid water-reducing agent produced by Jiangsu Subote New Materials Co., Ltd., with a water reduction rate of 32%, a solid content of 40%, and a dosage of 3.2 kg;

[0039] Microscopic energy-consuming components: 30kg of calcium carbonate whiskers with a length of 30μm and a diameter of 1μm produced by Lingshou County Tuyun Mineral Products Processing Plant, and 40kg of calcium sulfate whiskers with a length of 40μm and a diameter of 1.2μm produced by Hebei Ruijiang Metal Co., Ltd.

[0040] Looking at the energy-consuming components: the polyvinyl alcohol fiber with a length of 12 mm and a diameter of 39 μm produced by Shanghai Yingjia Industrial Development Co., Ltd. has a breaking elongation of 7.5% and a dosage of 15 kg; the alkali-resistant glass fiber with a length of 12 mm and a diameter of 14 μm produced by Shandong Hengtai New Materials Technology Co., Ltd. has a breaking elongation of 3.5% and a dosage of 35 kg;

[0041] Alkali-free accelerating setting agent: ZTSN-1 alkali-free accelerating setting agent produced by Anhui Zhongtie Engineering Materials Technology Co., Ltd., with a setting time of 3.5 minutes for the net slurry and a retention rate of 108% for 90d compressive strength, and a dosage of 80kg;

[0042] Water: Ordinary tap water, the dosage is 400kg.

[0043] Example 2

[0044] High-toughness cement-based materials for tunnel spraying construction with large deformation of surrounding rock, raw materials and 1m 3 The dosage of high toughness material is as follows:

[0045] Portland cement: Beijing Jinyu P·O 52.5 cement that meets the requirements of GB / 175-2007, with a dosage of 700kg;

[0046] Cave slag sand powder: The parent rock is marble with a uniaxial saturated compressive strength of 42.5MPa, the maximum particle size of the sand powder is 0.6mm, the crushing index is 6.5%, the MB value is 0.9g / kg, and the dosage is 550kg;

[0047] Working performance control material: ZTPCE-1 viscosity-reducing polycarboxylate water-reducing agent produced by Anhui Zhongtie Engineering Materials Technology Co., Ltd., with a water reduction rate of 35%, a solid content of 20%, and a dosage of 4.2kg;

[0048] Microscopic energy-consuming components: 40 kg of calcium carbonate whiskers with a length of 18 μm and a diameter of 0.5 μm produced by Lingshou County Tuyun Mineral Products Processing Plant, and 50 kg of calcium sulfate whiskers with a length of 40 μm and a diameter of 1 μm produced by Hebei Ruijiang Metal Co., Ltd.

[0049] Looking at the energy-consuming components in detail: the polyvinyl alcohol fiber produced by Japan Kuraray Co., Ltd. has a length of 12mm and a diameter of 8μm, an elongation at break of 8.2%, and a dosage of 15kg; the alkali-resistant glass fiber produced by Shandong Hengtai New Materials Technology Co., Ltd. has a length of 12mm and a diameter of 14μm, an elongation at break of 3.5%, and a dosage of 15kg; the basalt fiber produced by Sichuan Aerospace Tuoda Basalt Fiber Co., Ltd. has a length of 18mm and a diameter of 10μm, an elongation at break of 3.1%, and a dosage of 15kg;

[0050] Alkali-free accelerating setting agent: ZTSN-1 alkali-free accelerating setting agent produced by Anhui Zhongtie Engineering Materials Technology Co., Ltd., with a setting time of 3.5 minutes for the net slurry and a retention rate of 108% for the 90d compressive strength, and a dosage of 100kg;

[0051] Water: Ordinary tap water, the dosage is 420kg.

[0052] Example 3

[0053] High-toughness cement-based materials for tunnel spraying construction with large deformation of surrounding rock, raw materials and 1m 3 The dosage of high toughness material is as follows:

[0054] Portland cement: Beijing Jinyu P·O 42.5 cement that meets the requirements of GB / 175-2007, with a dosage of 900kg;

[0055] Cave slag sand powder: The parent rock uniaxial saturated compressive strength of dolomite is 49.7MPa, the maximum particle size of the sand powder is 1.18mm, the crushing index is 8.5%, the MB value is 0.6g / kg, and the dosage is 320kg;

[0056] Working performance control material: PCEA-1 viscosity-reducing polycarboxylic acid water-reducing agent produced by Jiangsu Subote New Materials Co., Ltd., with a water reduction rate of 35%, a solid content of 20%, and a dosage of 4.7 kg;

[0057] Microscopic energy-consuming components: 40 kg of calcium carbonate whiskers with a length of 30 μm and a diameter of 1 μm produced by Lingshou County Tuyun Mineral Products Processing Plant, and 60 kg of calcium sulfate whiskers with a length of 40 μm and a diameter of 1.2 μm produced by Hebei Ruijiang Metal Co., Ltd.

[0058] The energy-consuming components are as follows: the polyvinyl alcohol fiber produced by Japan Kuraray Co., Ltd. has a length of 12 mm and a diameter of 8 μm, an elongation at break of 8.2%, and a dosage of 20 kg; the basalt fiber produced by Sichuan Aerospace Tuoda Basalt Fiber Co., Ltd. has a length of 18 mm and a diameter of 10 μm, an elongation at break of 3.1%, and a dosage of 35 kg;

[0059] Alkali-free accelerating setting agent: TKSN-2 alkali-free accelerating setting agent produced by China Railway Academy Group Corporation, with a setting time of 3.1 minutes for pure slurry and a retention rate of 110% for 90d compressive strength, and a dosage of 70kg;

[0060] Water: Ordinary tap water, the amount is 470kg.

[0061] The schemes of the above-mentioned embodiments 1-3 of the present invention adopt the following steps to prepare the high-toughness cement-based material of slag sand powder for jetting construction of tunnels with large surrounding rock deformation:

[0062] (1) Add silicate cement, slag sand powder and micro energy-consuming components into a mixer and dry mix for 2-3 minutes;

[0063] (2) adding working performance regulating materials and 90% of water;

[0064] (3) Add the microscopic energy-consuming components and the remaining water and stir rapidly for 3-5 minutes;

[0065] (4) Add an accelerator to obtain a high-toughness cement-based material for tunnel slag sand powder spraying construction with large surrounding rock deformation.

[0066] Test example

[0067] The cement-based materials prepared in Examples 1-3 were tested for initial setting time with reference to the Standard for Performance Test Methods of Ordinary Concrete Mixtures (GB / T 50080-2016). When the cement-based materials were cured to 28 days old, the initial crack strength, ultimate tensile strain and compressive strength of the cement-based materials were tested with reference to the Test Method for Mechanical Properties of High Ductility Fiber Reinforced Cement-Based Composite Materials (JC / T2461-2018). The electric flux of the cement-based materials was tested with reference to the Standard for Long-term Performance and Durability Test Methods of Ordinary Concrete (GB / T50082-2009). The bonding strength between the cement-based materials and concrete was tested with reference to the Technical Specification for Application of Sprayed Concrete (JGJT372-2016). The results are shown in Table 1.

[0068] Table 1

[0069]

[0070]

[0071] As can be seen from Table 1, the high-toughness cement-based material of the present invention has an initial crack strength between 3.5MPa and 6.2MPa, an ultimate tensile strain between 1.9% and 3.4%, a compressive strength between 39.7MPa and 48.8MPa, and good toughness, which meets the initial support deformation requirements of the tunnel under the condition of large deformation of the surrounding rock; the electric flux is less than 1500C, and the durability is good; the bonding strength with concrete meets the standard requirements, and is suitable for jetting construction of tunnels with large deformation of surrounding rocks in complex stress fields, and has significant economic and environmental benefits.

[0072] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A high-toughness cement-based material for tunnel construction with large deformation of surrounding rock, characterized in that: The invention comprises the following raw materials in parts by weight: 600-1000 parts of silicate cement, 300-600 parts of slag sand powder, 50-100 parts of micro energy-consuming components, 20-60 parts of meso energy-consuming components, 60-100 parts of accelerating setting agent, 2-5 parts of working performance regulating material and 350-500 parts of water.

2. According to claim 1, a high-toughness cement-based material for tunnel spraying construction with large deformation of surrounding rock, characterized in that: The parent rock of the cave slag sand powder is hard rock, and the uniaxial saturated compressive strength of the hard rock is 30-60MPa.

3. A high-toughness cement-based material for tunnel construction with large deformation of surrounding rock according to claim 1 or 2, characterized in that: The particle size of the slag sand powder is less than 2.36 mm, the crushing index is less than 10%, and the MB value is less than 1.0 g / kg.

4. The high-toughness cement-based material of slag sand powder used for jetting construction of tunnels with large surrounding rock deformation according to claim 1 is characterized in that: The microscopic energy-consuming components are calcium carbonate whiskers and / or calcium sulfate whiskers; The whisker length in the micro energy-consuming component is 30-50 μm, and the aspect ratio is 20-40.

5. According to claim 1, a high-toughness cement-based material for tunnel jetting construction with large deformation of surrounding rock, characterized in that: The microscopic energy dissipation component is a mixture of any two or three of polyvinyl alcohol fiber, basalt fiber and alkali-resistant glass fiber.

6. The high-toughness cement-based material of slag sand powder used for jetting construction of tunnels with large surrounding rock deformation according to claim 5, characterized in that: The fiber monofilament used in the microscopic energy dissipation component has a length of 8-30 mm, an aspect ratio of 200-2000, and a breaking elongation greater than 3%.

7. The high-toughness cement-based material of slag sand powder used for jetting construction of tunnels with large surrounding rock deformation according to claim 5, characterized in that: The microscopic energy dissipation component is obtained by mixing polyvinyl alcohol fiber, basalt fiber and alkali-resistant glass fiber in a mass ratio of 20%-40%: 20%-80%: 20%-80%.

8. The high-toughness cement-based material of slag sand powder used for jetting construction of tunnels with large surrounding rock deformation according to claim 1, characterized in that: The working performance regulating material is a viscosity-reducing polycarboxylic acid water-reducing agent with a water-reducing rate greater than 30%.

9. The high-toughness cement-based material of slag sand powder used for jetting construction of tunnels with large surrounding rock deformation according to claim 1, characterized in that: The quick-setting agent is an alkali-free quick-setting agent, and the final setting time of the net slurry of the alkali-free quick-setting agent is less than 5 minutes, and the 90d compressive strength retention rate is greater than 105%.

10. The method for preparing high-toughness cement-based material of slag sand powder for jetting construction of tunnels with large surrounding rock deformation according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Add silicate cement, slag sand powder and micro energy-consuming components into a mixer and dry mix for 2-3 minutes; (2) adding working performance regulating materials and 90% of water; (3) Add the microscopic energy-consuming components and the remaining water and stir rapidly for 3-5 minutes; (4) Add an accelerator to obtain a high-toughness cement-based material for tunnel slag sand powder spraying construction with large surrounding rock deformation.

Citation Information

Patent Citations

  • High-toughness cement-based composite material and preparation method thereof

    CN114751701A

  • Tunnel jet type high-ductility concrete material and preparation method thereof

    CN115594479A

  • Concrete adopting granite tunneling hole slag as aggregate and used for underground engineering construction and preparation method thereof

    CN116023097A

  • Preparation process of concrete with tunnel slag as raw material

    CN116768538A