Lightweight high-strength concrete as well as preparation method and application thereof
Through the combination of ore powder, fly ash, silica fume compound, modified plant fibers, quartz sand, PE plastic particles, hollow glass microbeads and nanometal oxides, the problem of insufficient strength of traditional light aggregate concrete is solved. It realizes lightweight and high-strength concrete with low volume and high strength, suitable for floating bridges or floating boards.
Patent Information
- Application Number
- CN202411090958.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional light aggregate concrete is difficult to meet high-strength requirements due to the low strength of ceramic sand and drift beads. The brittle materials of ceramic sand need to increase the amount of additives to configure high-strength concrete with lower bulk weight and higher strength, but this will reduce the overall strength and make it difficult to Meet the requirements of lightweight and high strength.
Use ore powder, fly ash and silica fume as gelling materials to optimize particle grading to improve strength; use modified plant fibers to improve bonding strength between fiber and concrete matrix; quartz sand, PE plastic particles, hollow Glass microbead composite achieves low bulk weight and high strength; nanometal oxides are added for filling effect, enhance concrete strength, and reduce water absorption through methyl silicone oil.
Lightweight high-strength concrete with a volume weight of 1562~1687kg/m3 and a compressive strength of 153~160MPa is prepared. It is suitable for floating bridges or floating plates and meets structural strength requirements.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of building materials, and in particular to a lightweight high-strength concrete and a preparation method and application thereof. Background Art
[0002] Concrete is widely used in the construction and transportation industries due to its high strength and durability. With the continuous development of the concrete industry, high-strength and high-performance concrete has emerged in an endless stream. However, ordinary concrete uses sand and gravel as aggregates, and its apparent density is relatively high. When poured in large-sized structural parts or super-high-rise buildings, it has the disadvantages of heavy weight and high pumping difficulty. Traditional lightweight aggregate concrete uses ceramsite and ceramic sand as aggregates, and its bulk density is basically 1800kg / m 3 As mentioned above, due to the low strength of ceramsite and ceramic sand, the strength of the prepared lightweight aggregate concrete is limited and it is difficult to meet the relevant structural strength requirements. Lightweight high-strength concrete has gradually attracted attention and research. Patent CN107935505A uses fly ash beads and ceramic sand to prepare lightweight ultra-high-strength concrete with a bulk density greater than 1980kg / m 3 The compressive strength is between 105 and 111 MPa. However, the strength of ceramic sand and floating beads is generally not high, and ceramic sand is a brittle material. It is necessary to increase the dosage of the two to configure high-strength concrete with lower bulk density and higher strength, but this will reduce the overall strength, so it is difficult to meet the requirements of light weight and high strength. Summary of the invention
[0003] The object of the present invention is to provide a lightweight high-strength concrete and a preparation method and application thereof. The concrete has low bulk density and high strength and can be used for a floating slab or a floating bridge.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a lightweight high-strength concrete, comprising the following raw materials in parts by weight:
[0006] 200-300 parts of cement, 100-120 parts of fly ash, 60-100 parts of mineral powder, 40-60 parts of silica fume, 150-200 parts of lightweight ceramsite, 160-180 parts of modified lightweight aggregate, 20-40 parts of water reducer, 15-20 parts of modified plant fiber, 30-50 parts of quartz sand, 30-50 parts of PE plastic particles, 30-50 parts of hollow glass microspheres, 15-30 parts of nano-scale metal oxides, 30-50 parts of methyl silicone oil and 200-400 parts of water;
[0007] The modified lightweight aggregate is bentonite and desulfurized gypsum modified lightweight aggregate;
[0008] The modified plant fiber is silicon dioxide modified plant fiber.
[0009] Preferably, the lightweight aggregate in the modified lightweight aggregate includes one or more of pumice, fly ash ceramsite, shale ceramsite and expanded perlite.
[0010] Preferably, the preparation method of the modified lightweight aggregate comprises: mixing bentonite, desulfurized gypsum and lightweight aggregate, adding water under stirring conditions, and modifying to obtain the modified lightweight aggregate.
[0011] Preferably, the mass ratio of the lightweight aggregate to the total mass of bentonite and desulfurized gypsum is 15-30:1; the mass ratio of the bentonite to the desulfurized gypsum is 1:1-2.
[0012] Preferably, the method for preparing the modified plant fiber comprises:
[0013] The plant fiber is immersed in a sodium hydroxide solution for pretreatment, and then dried to obtain pretreated plant fiber;
[0014] Nano-sized silicon dioxide SiO 2 The solution is mixed with the pretreated plant fiber and modified to obtain modified plant fiber.
[0015] Preferably, the mass of the plant fiber is 60-70% of the mass of the sodium hydroxide solution; the pretreatment time is 6-10 hours; the modification time is 6-10 hours; the nano-scale silicon dioxide SiO 2 The mass ratio of the solution to the pretreated plant fiber is 0.6-0.8:1.
[0016] Preferably, the apparent density of the PE plastic particles is 0.91 to 0.97 g / cm 3 ;
[0017] The hollow glass microspheres contain SiO 2 The content is not less than 95wt%, and the apparent density is 460~480kg / m 3 , particle size D 50 Not more than 20μm, compressive strength not less than 110MPa;
[0018] The water reducing agent is a polyether polycarboxylic acid water reducing agent with a solid content of 18.9-20.1% and a water reducing rate of 35-40%.
[0019] Preferably, the nano-scale metal oxide includes nano-zirconium oxide or nano-titanium dioxide.
[0020] The present invention provides a method for preparing the lightweight high-strength concrete described in the above technical solution, comprising the following steps:
[0021] The cement, fly ash, mineral powder, silica fume, lightweight ceramsite and modified lightweight aggregate are first mixed to obtain a first mixed material;
[0022] Performing a second mixing of the first mixed material, water and a water reducing agent to obtain a second mixed material;
[0023] The second mixed material is mixed with modified plant fiber, quartz sand, PE plastic particles, hollow glass microspheres, nano-scale metal oxides and methyl silicone oil for a third time, and then formed and cured in water at a constant temperature to obtain lightweight and high-strength concrete.
[0024] The present invention provides the use of the lightweight high-strength concrete described in the above technical solution or the lightweight high-strength concrete prepared by the preparation method described in the above technical solution in a floating bridge or a floating slab.
[0025] The invention provides a lightweight high-strength concrete, comprising the following raw materials in parts by weight: 200-300 parts of cement, 100-120 parts of fly ash, 60-100 parts of mineral powder, 40-60 parts of silica fume, 150-200 parts of lightweight ceramsite, 160-180 parts of modified lightweight aggregate, 20-40 parts of water reducer, 15-20 parts of modified plant fiber, 30-50 parts of quartz sand, 30-50 parts of PE plastic particles, 30-50 parts of hollow glass microspheres, 15-30 parts of nano-scale metal oxides, 30-50 parts of methyl silicone oil and 200-400 parts of water; the modified lightweight aggregate is bentonite and desulfurized gypsum modified lightweight aggregate; the modified plant fiber is silicon dioxide modified plant fiber. The present invention uses a compound of mineral powder, fly ash and silica fume as a cementitious material, optimizes the particle gradation of the cementitious material, achieves close stacking and improves strength; uses modified plant fibers to improve the bonding strength between the fibers and the concrete matrix; uses a compound of quartz sand, PE plastic particles and hollow glass microspheres to achieve low bulk density and high strength; adds nano-metal oxides to achieve a good filling effect and enhance the strength of concrete; and adds methyl silicone oil to reduce the water absorption of concrete, thereby improving the structural strength of concrete. The lightweight concrete of the present invention is lightweight and high-strength, with a bulk density of 1562-1687kg / m 3 , the strength reaches 153 ~ 160MPa, and can be used for floating bridges or floating boards. DETAILED DESCRIPTION
[0026] The present invention provides a lightweight high-strength concrete, comprising the following raw materials in parts by weight:
[0027] 200-300 parts of cement, 100-120 parts of fly ash, 60-100 parts of mineral powder, 40-60 parts of silica fume, 150-200 parts of lightweight ceramsite, 160-180 parts of modified lightweight aggregate, 20-40 parts of water reducer, 15-20 parts of modified plant fiber, 30-50 parts of quartz sand, 30-50 parts of PE plastic particles, 30-50 parts of hollow glass microspheres, 15-30 parts of nano-scale metal oxides, 30-50 parts of methyl silicone oil and 200-400 parts of water;
[0028] The modified lightweight aggregate is bentonite and desulfurized gypsum modified lightweight aggregate;
[0029] The modified plant fiber is silicon dioxide modified plant fiber.
[0030] In terms of mass fraction, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 200 to 300 parts of cement, preferably 220 to 280 parts, and more preferably 250 to 260 parts. In the present invention, the cement is preferably silicate cement, and the silicate cement is preferably P·I52.5 cement, which has a specific surface area of 390m 2 / kg, 28-day compressive strength ≥52.5MPa, more preferably 59Mpa.
[0031] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 100 to 120 parts of fly ash, preferably 105 to 115 parts, and more preferably 110 parts. In the present invention, the fly ash is preferably Class I fly ash with a 45 μm square hole sieve residue of no more than 12% and a loss on ignition of no more than 5%.
[0032] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 60 to 100 parts of mineral powder, preferably 65 to 90 parts, and more preferably 70 to 80 parts. The mineral powder of the present invention preferably has a particle size distribution of 1 to 13 μm, D 50 The particle size is 3-5 μm, and the specific surface area is 800-1000 m 2 / kg of S105 grade mineral powder.
[0033] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 40 to 60 parts of silica fume, preferably 45 to 55 parts, and more preferably 50 parts. In the present invention, the specific surface area of the silica fume is preferably ≥ 22000m 2 / kg,SiO 2 The content is 85-95%.
[0034] The present invention adopts mineral powder, fly ash and silica fume cementitious materials to optimize particle gradation, achieve close stacking and improve strength.
[0035] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 150 to 200 parts of lightweight ceramsite, preferably 160 to 180 parts, and more preferably 165 to 175 parts. In the present invention, the particle size of the lightweight ceramsite is preferably 15 to 31.5 mm, and the bulk density is preferably 300 to 310 kg / m 3 .
[0036] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 160 to 180 parts of modified lightweight aggregate, preferably 165 to 175 parts, and more preferably 170 parts. In the present invention, the lightweight aggregate in the modified lightweight aggregate preferably includes one or more of pumice, fly ash ceramsite, shale ceramsite and expanded perlite; when the lightweight aggregate is two or more of the above, the present invention has no special restrictions on the ratio of different types of lightweight aggregates, and any ratio is acceptable. The present invention has no special restrictions on the source and specifications of the lightweight aggregate, and it can be obtained from commercially available products or well-known sources known in the art.
[0037] In the present invention, the preparation method of the modified lightweight aggregate preferably comprises: mixing bentonite, desulfurized gypsum and lightweight aggregate, adding water under stirring conditions, and performing modification to obtain the modified lightweight aggregate.
[0038] The present invention has no special limitation on the sources and composition of the bentonite and desulfurized gypsum, and they can be obtained from commercial products or well-known sources known in the art.
[0039] In the present invention, the ratio of the mass of the light aggregate to the total mass of bentonite and desulfurized gypsum is preferably 15 to 30:1; the mass ratio of the bentonite to the desulfurized gypsum is preferably 1:1 to 2; the mass of the water is preferably 8 to 15% of the mass of the light aggregate, and more preferably 10 to 15%. The present invention has no special restrictions on the mixing and stirring rates, as long as the materials are fully mixed. The present invention uses bentonite and desulfurized gypsum to improve the light aggregate, reduce the influence of the pores of the light aggregate on the concrete bonding process, and improve the strength of the concrete.
[0040] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 20 to 40 parts of a water reducer, preferably 25 to 35 parts, and more preferably 30 parts. In the present invention, the water reducer is preferably a polyether polycarboxylic acid water reducer, the solid content is preferably 18.9 to 20.1%, and the water reduction rate is preferably 35 to 40%.
[0041] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 15 to 20 parts of modified plant fibers, preferably 16 to 18 parts, and more preferably 17 parts.
[0042] In the present invention, the method for preparing the modified plant fiber preferably comprises:
[0043] The plant fiber is immersed in a sodium hydroxide solution for pretreatment, and then dried to obtain pretreated plant fiber;
[0044] Nano-sized silicon dioxide SiO 2 The solution is mixed with the pretreated plant fiber and modified to obtain modified plant fiber.
[0045] In the present invention, the plant fiber preferably includes one or more of sisal fiber, jute fiber, ramie fiber and flax fiber, bamboo fiber and cellulose fiber; when the plant fiber is more than two of the above types, the present invention has no special limitation on the ratio of different types of plant fibers, and any ratio is acceptable.
[0046] In the present invention, the mass of the plant fiber is preferably 60-70% of the mass of the sodium hydroxide solution, and more preferably 65%; the sodium hydroxide solution is preferably an aqueous sodium hydroxide solution, and the concentration of the aqueous sodium hydroxide solution is preferably 2-5wt%, and more preferably 3-4wt%; the pretreatment time is preferably 6-10h, and more preferably 7-9h; after the pretreatment is completed, the plant fiber is taken out, washed with water, and naturally air-dried to obtain modified plant fiber.
[0047] In the present invention, the nano-scale silicon dioxide SiO 2 The concentration of the solution is preferably 3-5wt%, more preferably 3.5-4.0wt%; the nano-scale silicon dioxide SiO 2 The mass ratio of the solution to the pretreated plant fiber is preferably 0.6-0.8:1, more preferably 0.65-0.75:1, and further preferably 0.7:1; the modification time is preferably 6-10 hours, more preferably 7-8 hours, and the pressure is preferably 50-60 MPa, more preferably 55 MPa.
[0048] After the modification is completed, the present invention preferably naturally dries the obtained product to obtain modified plant fiber.
[0049] The present invention modifies the surface of plant fibers, improves the bonding strength between the fibers and the concrete matrix, and thus improves the strength of the concrete.
[0050] Based on the mass fraction of the cement, the raw material for preparing the lightweight high-strength concrete provided by the present invention includes 30 to 50 parts of quartz sand, preferably 35 to 45 parts, and more preferably 40 parts. In the present invention, the density of the quartz sand is preferably 2.20 to 2.66 g / cm 3 The present invention utilizes quartz sand to improve the strength, acid resistance and durability of concrete.
[0051] Based on the mass fraction of the cement, the raw material for preparing the lightweight high-strength concrete provided by the present invention includes 30 to 50 parts of PE plastic particles, preferably 35 to 45 parts, and more preferably 40 parts. In the present invention, the apparent density of the PE plastic particles is preferably 0.91 to 0.97 g / cm 3 .
[0052] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 30 to 50 parts of hollow glass microspheres, preferably 35 to 45 parts, and more preferably 40 parts. In the present invention, the SiO 2 The content is preferably not less than 95wt%, and the apparent density is preferably 460-480kg / m 3 , particle size D 50 The thickness is preferably not greater than 20 μm, and the compressive strength is preferably not less than 110 MPa.
[0053] The invention utilizes quartz sand, PE plastic particles and hollow glass microspheres to achieve the purpose of low bulk density and high overall strength.
[0054] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 15 to 30 parts of nano-scale metal oxides, preferably 20 to 28 parts, and more preferably 23 to 25 parts. In the present invention, the nano-scale metal oxide preferably includes nano-zirconia or nano-titanium dioxide. The present invention does not specifically limit the specifications of the nano-zirconia or nano-titanium dioxide, and commercial products well known in the art can be used. The present invention utilizes nano-scale metal oxides to achieve a good filling effect and enhance the strength of concrete.
[0055] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 30 to 50 parts of methyl silicone oil, preferably 35 to 45 parts, and more preferably 40 parts. The present invention utilizes methyl silicone oil to reduce the water absorption rate of concrete, thereby improving the structural strength of concrete.
[0056] Based on the mass fraction of the cement, the raw materials for preparing the lightweight high-strength concrete provided by the present invention include 200 to 400 parts of water.
[0057] The present invention provides a method for preparing the lightweight high-strength concrete described in the above technical solution, comprising the following steps:
[0058] The cement, fly ash, mineral powder, silica fume, lightweight ceramsite and modified lightweight aggregate are first mixed to obtain a first mixed material;
[0059] Performing a second mixing of the first mixed material, water and a water reducing agent to obtain a second mixed material;
[0060] The second mixed material is mixed with modified plant fiber, quartz sand, PE plastic particles, hollow glass microspheres, nano-scale metal oxides and methyl silicone oil for a third time, and then formed and cured in water at a constant temperature to obtain lightweight and high-strength concrete.
[0061] In the present invention, the first mixing time is preferably 20 to 30 minutes; the second mixing time is preferably 15 to 30 minutes; the third mixing time is preferably 10 to 15 minutes. The present invention has no particular limitation on the stirring rate of the mixing, and the materials can be fully mixed according to the process well known in the art.
[0062] In the present invention, the mold is preferably removed after 24 hours of molding at room temperature, and the water curing temperature is preferably 60-80° C., and the time is preferably 28 days.
[0063] The present invention provides the application of the lightweight high-strength concrete described in the above technical solution or the lightweight high-strength concrete prepared by the preparation method described in the above technical solution in a floating bridge or a floating slab. The present invention has no special limitation on the application method, and the application can be carried out according to methods well known in the art.
[0064] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0065] In the following examples, cement is P·I52.5 silicate cement with a specific surface area of 390m 2 / kg, 28-day compressive strength is 59Mpa;
[0066] The fly ash is Class I fly ash with a 45μm square mesh sieve residue of no more than 12% and a loss on ignition of no more than 5%;
[0067] The particle size distribution of mineral powder is 1~13μm, D 50 The particle size is 3-5 μm, and the specific surface area is 800-1000 m 2 / kg of S105 grade mineral powder;
[0068] The specific surface area of silica fume is 23500m 2 / kg,SiO 2 The content is 92%;
[0069] The particle size of lightweight ceramsite is 15-31.5mm, and the bulk density is 300-310kg / m 3 ;
[0070] The water reducing agent is a polyether polycarboxylic acid water reducing agent with a solid content of 19.8% and a water reducing rate of 40%.
[0071] Example 1
[0072] The lightweight high-strength concrete provided by the present invention comprises the following raw materials in parts by weight:
[0073] 300 parts of cement, 120 parts of fly ash, 80 parts of mineral powder, 50 parts of silica fume, 180 parts of lightweight ceramsite, 170 parts of modified lightweight aggregate, 20 parts of water reducer, 16 parts of modified plant fiber, 35 parts of quartz sand, 40 parts of PE plastic particles, 45 parts of hollow glass microspheres, 20 parts of nano zirconium oxide, 35 parts of methyl silicone oil and 350 parts of water;
[0074] Preparation of modified light aggregate: bentonite, desulfurized gypsum and light aggregate (pumice, particle size 6-10 mm) are mixed, and water is added under stirring conditions to modify the light aggregate to obtain modified light aggregate; the mass ratio of the light aggregate to the total mass of bentonite and desulfurized gypsum is 20:1; the mass ratio of the bentonite to the desulfurized gypsum is 1:1; the mass of water is 12% of the mass of the light aggregate;
[0075] Preparation method of modified plant fiber:
[0076] The plant fiber (bamboo fiber) is immersed in a 3 wt % sodium hydroxide aqueous solution for 8 hours, and then the plant fiber is taken out, washed with water, and naturally air-dried to obtain a pretreated plant fiber;
[0077] The concentration of 5wt% nano-silicon dioxide SiO 2 The solution is mixed with the pretreated plant fiber, modified under a pressure of 60 MPa for 8 hours, and the obtained product is naturally dried to obtain modified plant fiber; the mass of the plant fiber is 65% of the mass of the sodium hydroxide solution; the nano-scale silicon dioxide SiO 2 The mass ratio of solution to pretreated plant fiber was 0.7:1;
[0078] Preparation method of lightweight and high-strength concrete:
[0079] The cement, fly ash, mineral powder, silica fume, lightweight ceramsite and modified lightweight aggregate are first mixed for 30 minutes to obtain a first mixed material;
[0080] The first mixed material is mixed with water and a water reducing agent for a second time for 30 minutes to obtain a second mixed material;
[0081] The second mixed material was mixed with modified plant fiber, quartz sand, PE plastic particles, hollow glass microspheres, nano-scale metal oxides and methyl silicone oil for a third time for 15 minutes, and then the mold was removed after molding for 24 hours, and the concrete was cured in water at a constant temperature of 70° C. for 28 days to obtain a lightweight and high-strength concrete.
[0082] Example 2
[0083] The lightweight high-strength concrete provided by the present invention comprises the following raw materials in parts by weight:
[0084] 200 parts of cement, 110 parts of fly ash, 60 parts of mineral powder, 60 parts of silica fume, 150 parts of lightweight ceramsite, 160 parts of modified lightweight aggregate, 30 parts of water reducer, 15 parts of modified plant fiber, 30 parts of quartz sand, 50 parts of PE plastic particles, 30 parts of hollow glass microspheres, 30 parts of nano titanium dioxide, 30 parts of methyl silicone oil and 400 parts of water;
[0085] Preparation of modified lightweight aggregate: Bentonite, desulfurized gypsum and lightweight aggregate (fly ash ceramsite, particle size 5-15mm, density 630-700kg / m 3 ) and adding water under stirring to modify the material to obtain a modified light aggregate; the mass ratio of the light aggregate to the total mass of bentonite and desulfurized gypsum is 15:1; the mass ratio of the bentonite to the desulfurized gypsum is 1:2; the mass of water is 15% of the mass of the light aggregate;
[0086] Preparation method of modified plant fiber:
[0087] The plant fiber (flax fiber) is immersed in a 5 wt % sodium hydroxide aqueous solution for 6 hours, and then the plant fiber is taken out, washed with water, and naturally air-dried to obtain a pretreated plant fiber;
[0088] The concentration of 3wt% nano-silicon dioxide SiO 2 The solution is mixed with the pretreated plant fiber, modified for 6 hours under a pressure of 50 MPa, and the obtained product is naturally dried to obtain modified plant fiber; the mass of the plant fiber is 70% of the mass of the sodium hydroxide solution; the nano-scale silicon dioxide SiO 2 The mass ratio of solution to pretreated plant fiber was 0.8:1;
[0089] Preparation method of lightweight and high-strength concrete:
[0090] The cement, fly ash, mineral powder, silica fume, lightweight ceramsite and modified lightweight aggregate are first mixed for 30 minutes to obtain a first mixed material;
[0091] The first mixed material is mixed with water and a water reducing agent for a second time for 30 minutes to obtain a second mixed material;
[0092] The second mixed material was mixed with modified plant fiber, quartz sand, PE plastic particles, hollow glass microspheres, nano-scale metal oxides and methyl silicone oil for a third time for 15 minutes, and the mold was removed after molding for 24 hours. The concrete was then cured in water at a constant temperature of 80° C. for 28 days to obtain a lightweight and high-strength concrete.
[0093] Example 3
[0094] The lightweight high-strength concrete provided by the present invention comprises the following raw materials in parts by weight:
[0095] 250 parts of cement, 100 parts of fly ash, 100 parts of mineral powder, 40 parts of silica fume, 200 parts of lightweight ceramsite, 180 parts of modified lightweight aggregate, 40 parts of water reducer, 20 parts of modified plant fiber, 50 parts of quartz sand, 30 parts of PE plastic particles, 50 parts of hollow glass microspheres, 15 parts of nano zirconium oxide, 50 parts of methyl silicone oil and 300 parts of water;
[0096] Preparation of modified light aggregate: bentonite, desulfurized gypsum and light aggregate (expanded perlite) are mixed, and water is added under stirring conditions to modify the light aggregate to obtain modified light aggregate; the mass ratio of the light aggregate to the total mass of bentonite and desulfurized gypsum is 30:1; the mass ratio of the bentonite to the desulfurized gypsum is 1:1; the mass of water is 8% of the mass of the light aggregate;
[0097] Preparation method of modified plant fiber:
[0098] After soaking plant fiber (sisal fiber) in a 2 wt % sodium hydroxide aqueous solution for 10 hours, the plant fiber is taken out, washed with water, and naturally air-dried to obtain pretreated plant fiber;
[0099] The concentration of 5wt% nano-silicon dioxide SiO 2 The solution is mixed with the pretreated plant fiber, modified for 6 hours under a pressure of 60 MPa, and the obtained product is naturally dried to obtain modified plant fiber; the mass of the plant fiber is 60% of the mass of the sodium hydroxide solution; the nano-scale silicon dioxide SiO 2 The mass ratio of solution to pretreated plant fiber was 0.6:1;
[0100] Preparation method of lightweight and high-strength concrete:
[0101] The cement, fly ash, mineral powder, silica fume, lightweight ceramsite and modified lightweight aggregate are first mixed for 20 minutes to obtain a first mixed material;
[0102] The first mixed material is mixed with water and a water reducing agent for a second time for 20 minutes to obtain a second mixed material;
[0103] The second mixed material was mixed with modified plant fiber, quartz sand, PE plastic particles, hollow glass microspheres, nano-scale metal oxides and methyl silicone oil for a third time for 10 minutes, and the mold was removed after molding for 24 hours. The concrete was then cured in water at a constant temperature of 60° C. for 28 days to obtain a lightweight and high-strength concrete.
[0104] Comparative Example 1
[0105] The only difference from Example 1 is that no mineral powder and silica fume are added, and the rest is the same as Example 1.
[0106] Comparative Example 2
[0107] The only difference from Example 1 is that no mineral powder and fly ash are added, and the rest is the same as Example 1.
[0108] Comparative Example 3
[0109] The only difference from Example 1 is that fly ash and silica fume are not added, and the rest is the same as Example 1.
[0110] Comparative Example 4
[0111] The only difference from Example 1 is that no modified plant fiber is added, and the rest is the same as Example 1.
[0112] Comparative Example 5
[0113] The only difference from Example 1 is that unmodified lightweight aggregate is added, and the rest is the same as Example 1.
[0114] Comparative Example 6
[0115] The only difference from Example 1 is that quartz sand, PE plastic particles and hollow glass microspheres are not added, and the rest is the same as Example 1.
[0116] Comparative Example 7
[0117] The only difference from Example 1 is that no nano zirconium oxide is added, and the rest is the same as Example 1.
[0118] Comparative Example 8
[0119] The only difference from Example 1 is that methyl silicone oil is not added, and the rest is the same as Example 1.
[0120] Performance Testing
[0121] The bulk density and compressive strength of the lightweight high-strength concrete in Examples 1-3 and Comparative Examples 1-7 were measured according to "Common Concrete Mechanics Test Method" CB50081-2002. The results are shown in Table 1:
[0122] Table 1 Test results of lightweight ultra-high strength concrete performance indicators
[0123] Case <![CDATA[Unit weight (kg / m 3 )]]> Compressive strength(MPa) Example 1 1562 160 Example 1 1635 153 Example 1 1687 155 Comparative Example 1 1691 146 Comparative Example 2 1693 147 Comparative Example 3 1689 135 Comparative Example 4 1694 136 Comparative Example 5 1701 133 Comparative Example 6 1705 130 Comparative Example 7 1703 143 Comparative Example 8 1706 145
[0124] As shown in Table 1, the concrete of the present invention has a bulk density of 1562-1687 kg / m 3 When the concrete is quartz crystal, the strength reaches 153-160MPa, which is a lightweight and high-strength concrete and can be used for floating bridges or floating slabs.
[0125] In addition, according to Table 1, by comparing Examples 1 to 3 with Comparative Examples 1 to 8, it can be seen that the compound use of mineral powder, silica fume and fly ash can improve the strength of concrete; modified plant fiber, modified lightweight aggregate, nano oxide and methyl silicone oil will affect the capacity and strength of concrete. The present invention adopts modified plant fiber, modified lightweight aggregate, nano oxide and methyl silicone oil to improve the capacity and strength of concrete.
[0126] Moreover, the compound use of quartz sand, PE plastic particles and hollow glass microspheres can also improve the strength of concrete.
[0127] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A lightweight high-strength concrete, characterized in that: The preparation comprises the following raw materials in parts by weight: 200-300 parts of cement, 100-120 parts of fly ash, 60-100 parts of mineral powder, 40-60 parts of silica fume, 150-200 parts of lightweight ceramsite, 160-180 parts of modified lightweight aggregate, 20-40 parts of water reducer, 15-20 parts of modified plant fiber, 30-50 parts of quartz sand, 30-50 parts of PE plastic particles, 30-50 parts of hollow glass microspheres, 15-30 parts of nano-scale metal oxides, 30-50 parts of methyl silicone oil and 200-400 parts of water; The modified lightweight aggregate is bentonite and desulfurized gypsum modified lightweight aggregate; The modified plant fiber is silicon dioxide modified plant fiber.
2. The lightweight high-strength concrete according to claim 1, characterized in that: The light aggregate in the modified light aggregate includes one or more of pumice, fly ash ceramsite, shale ceramsite and expanded perlite.
3. The lightweight high-strength concrete according to claim 1, characterized in that: The preparation method of the modified light aggregate comprises: mixing bentonite, desulfurized gypsum and light aggregate, adding water under stirring conditions, performing modification, and obtaining the modified light aggregate.
4. The lightweight high-strength concrete according to claim 3, characterized in that: The mass ratio of the lightweight aggregate to the total mass of bentonite and desulfurized gypsum is 15-30:1; the mass ratio of the bentonite to desulfurized gypsum is 1:1-2.
5. The lightweight high-strength concrete according to claim 1, characterized in that: The preparation method of the modified plant fiber comprises: The plant fiber is immersed in a sodium hydroxide solution for pretreatment, and then dried to obtain pretreated plant fiber; The nano-scale silicon dioxide SiO2 solution is mixed with the pretreated plant fiber and modified to obtain the modified plant fiber.
6. The lightweight high-strength concrete according to claim 5, characterized in that: The mass of the plant fiber is 60-70% of the mass of the sodium hydroxide solution; the pretreatment time is 6-10 hours; the modification time is 6-10 hours; the mass ratio of the nano-scale silicon dioxide SiO2 solution to the pretreated plant fiber is 0.6-0.8:
1.
7. The lightweight high-strength concrete according to claim 1, characterized in that: The apparent density of the PE plastic particles is 0.91-0.97 g / cm 3 ; The SiO2 content of the hollow glass microspheres is not less than 95wt%, and the apparent density is 460-480kg / m 3 , particle size D 50 Not more than 20μm, compressive strength not less than 110MPa; The water reducing agent is a polyether polycarboxylic acid water reducing agent with a solid content of 18.9-20.1% and a water reducing rate of 35-40%.
8. The lightweight high-strength concrete according to claim 1, characterized in that: The nano-scale metal oxide includes nano-zirconium oxide or nano-titanium dioxide.
9. The method for preparing the lightweight high-strength concrete according to claims 1 to 8, characterized in that: The following steps are involved: The cement, fly ash, mineral powder, silica fume, lightweight ceramsite and modified lightweight aggregate are first mixed to obtain a first mixed material; Performing a second mixing of the first mixed material, water and a water reducing agent to obtain a second mixed material; The second mixed material is mixed with modified plant fiber, quartz sand, PE plastic particles, hollow glass microspheres, nano-scale metal oxides and methyl silicone oil for a third time, and then formed and cured in water at a constant temperature to obtain lightweight and high-strength concrete.
10. Use of the lightweight high-strength concrete according to any one of claims 1 to 8 or the lightweight high-strength concrete prepared by the preparation method according to claim 9 in floating bridges or floating slabs.
Citation Information
Patent Citations
Light low-shrinkage super-high performance concrete and preparation method thereof
CN107935505A
Cited By
DEF inhibition filler, anti-crack UHPC, and preparation method and application of anti-crack UHPC
CN120172670A