Spinel structure high-entropy ceramic aerogel material as well as preparation method and application thereof

By using hydrated metal inorganic salts and gel accelerators to prepare spinel structure high-entropy ceramic aerogel materials, the problems of complex preparation process of existing high-entropy ceramic materials and instability of aerogel materials are solved, and components are uniform. The structure is stable with high specific surface area and low high temperature thermal conductivity, suitable for extreme heat insulation and high temperature resistant materials.

CN118978395APending Publication Date: 2024-11-19NANCHANG HANGKONG UNIVERSITY

Patent Information

Application Number
CN202411057884.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The preparation process of existing high-entropy ceramic materials is cumbersome, with long cycles and high equipment requirements, and the particle size is difficult to control during sintering, resulting in limited industrial promotion, and the preparation method of aerogel materials is difficult to target a variety of precursors and components. Unevenness, unstable gel structure.

Method used

The hydrated metal inorganic salt is used as the cation source, and the metal ion precursor solution is formed by uniform mixing solvents, and a gel accelerator is added to form a wet gel. After aging and drying at normal pressure, a spinel structure high-entropy ceramic aerogel is obtained. Material.

Benefits of technology

The spinel structure high-entropy ceramic aerogel material has uniform components and stable structure, and has excellent performance with high specific surface area and low high temperature thermal conductivity. It simplifies the preparation process and reduces costs. It is suitable for extreme heat insulation and resistance. High temperature material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978395A_ABST
    Figure CN118978395A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ceramic aerogel materials, and provides a spinel-structured high-entropy ceramic aerogel material and a preparation method and application thereof.The preparation method comprises the steps that hydrated metal inorganic salt serves as a cation source, and deionized water and an organic solvent are used for dissolving the hydrated metal inorganic salt; the invention relates to a preparation method of a spinel-structured high-entropy ceramic aerogel material, which comprises the following steps of: preparing a metal ion precursor solution, uniformly mixing to form the metal ion precursor solution, forming wet gel under the action of a gel accelerator, aging, drying at normal pressure to form an aerogel precursor, and finally performing heat treatment to obtain the spinel-structured high-entropy ceramic aerogel material, and the preparation method is short in process flow, simple and convenient to operate, mild in condition, safe, efficient and low in cost. The prepared spinel-structured high-entropy ceramic aerogel material has a uniform nanoscale reticular porous structure, a relatively high specific surface area and a relatively low high-temperature heat conductivity coefficient, and is a reserve base material in the fields of extreme heat insulation and high temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic aerogel materials, and in particular relates to a spinel structure high entropy ceramic aerogel material and a preparation method and application thereof. Background Art

[0002] Spinel is a type of crystal with a simple structural formula of XY2O4. It has a face-centered cubic structure in the equiaxed crystal system. Due to its excellent properties such as high melting point, relatively low density, high hardness, high strength at room temperature and high temperature, thermal shock resistance, chemical corrosion resistance, wide energy band gap, high resistance and low thermal expansion coefficient, it has shown broad application prospects in optical transparent devices, neutron irradiation resistance, humidity sensors, refractory materials, catalysis and catalyst carriers. In the spinel structure, oxygen ions are stacked in the normal direction of the (111) crystal plane in the order of abc, and the tetrahedral and octahedral layers are arranged alternately, while X ions only occupy 1 / 8 of the 64 tetrahedral vacancies, that is, 8 A sites, and Y ions only occupy 1 / 2 of the 32 octahedral vacancies, that is, 16 B sites. There are abundant interstitial sites in the spinel structure, which makes it possible to use the "high entropy" concept to design its structure and composition to obtain high-entropy ceramics with improved performance.

[0003] High-entropy ceramics are solid solutions with high configurational entropy formed by the combination of five or more cations or anions in equal or nearly equal molar amounts. They are a new type of multifunctional material developed in the direction of ceramic materials after the application of the concept of "configurational entropy stable single phase" in high-entropy alloys. Due to the uniqueness of the structure and the diversity of components, high-entropy ceramics exhibit high entropy effects in thermodynamics, lattice distortion effects in structure, hysteresis diffusion effects in kinetics, and "cocktail" effects in performance, which can improve the macroscopic properties of materials and are increasingly attracting research interest.

[0004] High-entropy ceramic materials are generally prepared by the solid-phase reaction method, which has complicated processes, lengthy cycles, and high requirements for equipment. Therefore, this method is not conducive to industrial promotion. At the same time, it is difficult to avoid abnormal growth of particle size during the sintering process.

[0005] Aerogel is a type of porous material composed of nano-scale solid particles and pores. The continuous three-dimensional network structure can be regulated and tailored at the nanoscale. Due to the fine porous structure, aerogel materials often have high specific surface areas (~1500m 2 / g), high porosity (~99.8%), ultra-low density (0.003~0.35g / cm 3Aerogel block materials are usually prepared by sol-gel method and supercritical drying technology, because different types of precursors have different reaction rates in the sol-gel reaction process, resulting in uneven components and unstable gel structure, so this preparation method can generally only be prepared for a single or two precursors. At the same time, the subsequent supercritical drying is limited by the high temperature, long cycle and high equipment requirements. Summary of the invention

[0006] In view of the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a spinel structure high entropy ceramic aerogel material and its preparation method and application. The present invention uses a hydrated metal inorganic salt as a cation source, uses a solvent to dissolve the hydrated metal inorganic salt, and uniformly mixes to form a metal ion precursor solution, and then forms a wet gel through the action of a gel promoter, and then forms an aerogel precursor through aging and normal pressure drying. Finally, the aerogel precursor is heat-treated to obtain a spinel structure high entropy ceramic aerogel material. The obtained spinel structure high entropy ceramic aerogel material has a uniform nanoscale mesh porous structure, its components are uniform, the gel structure is stable, and because it has the structure of an aerogel, it has the excellent properties of high specific surface area and low high-temperature thermal conductivity.

[0007] The present invention is achieved through the following technical solutions:

[0008] A spinel structure high entropy ceramic aerogel material, the spinel structure high entropy ceramic aerogel material expression is (Mg x1 Co x2 Ni x3 Cu x4 Zn x5)M2O4, x1, x2, x3, x4 and x5 are the ratios of the number of atoms, x1+x2+x3+x4+x5=1, 0.05≤x1≤0.35, 0.05≤x2≤0.35, 0.05≤x3≤0.35, 0.05≤x4≤0.35, 0.05≤x5≤0.35, M is one of Al, Cr, Mn and Fe. When x1, x2, x3, x4 and x5 exceed the upper limit of 0.35, it is not conducive to the formation of a stable high entropy single-phase solid solution, and when it is lower than the lower limit of 0.05, the high entropy effect is not obvious, so it is determined that 0.35≥x1, x2, x3, x4 and x5≥0.05. Mg, Co, Ni, Cu, and Zn have similar ionic radii and their divalent hydrated inorganic salts are readily available, and Al, Cr, Mn, and Fe trivalent hydrated inorganic salts are readily available. Therefore, the present invention selects divalent hydrated inorganic salts of Mg, Co, Ni, Cu, and Zn and trivalent hydrated inorganic salts of Al, Cr, Mn, and Fe as raw materials for preparation.

[0009] The present invention also provides a method for preparing a spinel structure high entropy ceramic aerogel material, comprising the following steps:

[0010] S1. Weigh five divalent hydrated inorganic salts of Mg, Co, Ni, Cu and Zn respectively, weigh one of the trivalent hydrated inorganic salts of Al, Cr, Mn and Fe, mix the five divalent hydrated inorganic salts with one trivalent hydrated inorganic salt to obtain a mixed inorganic salt; considering that the existing solid phase reaction method and supercritical drying technology have complex preparation processes and high energy consumption, and are difficult to use on a large scale, the present invention proposes to directly use a hydrated metal inorganic salt as a cation source in order to simplify the process, and dissolve the hydrated metal inorganic salt in a solvent, thereby facilitating the full and uniform mixing of metal cations;

[0011] Adding a solvent to the mixed inorganic salt and dispersing the mixed inorganic salt uniformly to obtain a metal ion precursor solution; the hydrated metal inorganic salt used to prepare the metal ion precursor solution is selected from nitrates, chlorates or sulfates;

[0012] In order to further ensure that the hydrated metal inorganic salt is completely dissolved and fully mixed, the present invention preferably adopts magnetic stirring or mechanical stirring to dissolve the hydrated metal inorganic salt in the solvent, and stirs at 20-50°C and 300-600rpm for 10-60min; too low temperature and speed will lead to too long stirring time, while too high temperature and speed will lead to excessive loss of solvent volatilization;

[0013] S2, adding a gel accelerator to the metal ion precursor solution, wherein the gel accelerator is an epoxy compound, and mixing them evenly, and standing until a gel transition occurs, so as to cause the metal ion precursor solution to undergo a polycondensation reaction to form a wet gel;

[0014] It should be noted that, in order to enable the metal ion precursor solution to be converted into a wet gel with a stable network skeleton structure, the present invention preferably adds a gel promoter of an epoxy compound, the epoxy compound is a proton capture agent, and under the action of metal cations, the epoxy compound undergoes an irreversible ring-opening reaction to form free radicals with high chemical activity. The presence of free radicals accelerates the reaction rate between hydrated metal cations, and at the same time, the pH of the metal ion precursor solution is adjusted to 9-12, and then the solution is allowed to stand, and the metal ions form hydrated ions in the aqueous solution. The hydrated ions are dehydrated and condensed in an alkaline environment by the standing treatment, thereby forming a wet gel with a stable structure;

[0015] In order to ensure that the gel accelerator can be evenly dispersed in the metal ion precursor solution, the present invention preferably continues stirring for 5 to 20 minutes at a temperature of 20 to 50° C. and a speed of 300 to 600 rpm;

[0016] In order to further ensure that during the standing process, the hydrated ions undergo dehydration condensation in an alkaline environment, thereby forming a wet gel with a stable network skeleton structure, the present invention preferably has a standing temperature of 20 to 60° C. and a standing time of 20 to 60 min.

[0017] The gel accelerator of the present invention is selected from one of propylene oxide, epoxybutene, cyclohexene oxide, glycidol, epifluoropropane, epichlorohydrin, epibromopropane and epitene oxide;

[0018] S3, subjecting the wet gel to an aging treatment, and then to washing and drying treatments to obtain an aerogel precursor;

[0019] In order to further enhance the network skeleton structure of the wet gel to form an aerogel material with a high specific surface area, the present invention first adds an aging agent to the wet gel, and soaks the wet gel with the aging agent to enhance the skeleton strength of the wet gel through the aging treatment;

[0020] In order to ensure that the added aging agent can achieve the above technical effects, the present invention preferably has a volume ratio of the wet gel to the aging agent of 1:2-3, wherein the aging agent is selected from one or more of methanol, ethanol, isopropanol, n-butanol, n-pentane, acetonitrile, and dimethylformamide;

[0021] Considering that the gel accelerator or its reaction product exists in the pores and surface of the material after aging treatment, washing is performed to achieve the purpose of removing the gel accelerator or its reaction product; and in order to ensure that the above technical effect can be achieved by washing, the present invention preferably uses anhydrous ethanol as a washing agent, and washes repeatedly for 3 to 5 times, with an interval of 10 to 30 minutes each time;

[0022] Considering the defect that the material after washing has pores filled with organic solvents and water liquid medium, atmospheric pressure drying is performed to achieve the purpose of replacing the liquid medium with the gas medium. In order to ensure that the above technical effects can be achieved by atmospheric pressure drying, the present invention preferably has a drying temperature of 80 to 150° C. and a drying time of 24 to 48 hours.

[0023] S4, heat-treating the aerogel precursor to obtain a spinel structure high entropy ceramic aerogel material; the aerogel precursor does not form a single-phase solid solution, so the purpose of preparing the spinel structure high entropy ceramic aerogel material is achieved through heat treatment.

[0024] Preferably, the molar ratio of the five divalent hydrated inorganic salts of Mg, Co, Ni, Cu and Zn is 1-7:1-7:1-7:1-7:1-7.

[0025] Preferably, the ratio of the total molar amount of five divalent hydrated inorganic salts to the molar amount of one trivalent hydrated inorganic salt is 0.5:1. When the usage ratio is lower than the lower limit, the configurational entropy of the reaction system decreases, thereby reducing the ability to form a high-entropy single phase; when the usage ratio is higher than the upper limit, the formed high-entropy single-phase structure is unstable.

[0026] Preferably, in order to ensure that the hydrated metal inorganic salt is fully and evenly mixed, the solvent consists of deionized water and an organic solvent, the organic solvent is selected from methanol, ethanol, isopropanol, n-butanol, n-pentane, acetonitrile or dimethylformamide, the molar ratio of the organic solvent to deionized water is 0.4-4:1, and the molar ratio of deionized water to the trivalent hydrated inorganic salt is 2-25:1. When the dosage ratio is lower than the lower limit, the hydrated metal inorganic salt cannot be completely dissolved and the mixing is uneven; when the dosage ratio is higher than the upper limit, the metal ion concentration is too low to form a stable gel structure.

[0027] Preferably, in order to ensure that the pH of the metal ion precursor solution can be adjusted to 9-12, the volume ratio of the gel accelerator substance to the solvent is 1.7-24 mol:1L.

[0028] Preferably, considering the defect of the wet gel having a weak network skeleton, an aging treatment is performed to achieve the purpose of enhancing the skeleton strength. The aging treatment method is: the wet gel is mixed with an aging agent and then sealed, and the aging treatment is performed at 40 to 65° C. for 24 to 72 hours.

[0029] Preferably, the heat treatment method is: keeping the temperature at 600-1200° C. in an air atmosphere for 1-2 hours, and then cooling to room temperature along with the furnace.

[0030] The present invention also protects the application of the spinel structure high entropy ceramic aerogel material in the preparation of thermal insulation materials or high temperature resistant materials.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. Aerogel is a type of porous material composed of nano-scale solid particles and pores, and the continuous three-dimensional network structure can be regulated and tailored at the nanoscale. The present invention proposes to use a sol-gel process to prepare a spinel structure high entropy ceramic aerogel. The obtained spinel structure high entropy ceramic aerogel material has a high specific area and a low high-temperature thermal conductivity, so that the obtained spinel structure high entropy ceramic aerogel material can be used in extreme heat insulation and high temperature resistance fields.

[0033] 2. The present invention provides a new preparation method for a spinel structure high entropy ceramic aerogel material, which uses a hydrated metal inorganic salt as a raw material. After the hydrated inorganic salt is completely dissolved, a gel promoter is added to allow the metal cations to undergo a dehydration condensation reaction in an alkaline solution to form a wet gel with uniform components and stable structure. The aerogel precursor is obtained by aging, washing and drying at normal pressure. Finally, the aerogel precursor is heat-treated to obtain a spinel structure high entropy ceramic aerogel material.

[0034] 3. The preparation method of the present invention has the advantages of short preparation cycle, simple process, low cost and low equipment requirements, and can be used for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a physical picture of the wet gel prepared in Example 1;

[0036] Figure 2 This is a physical picture of the spinel structure high entropy ceramic aerogel material prepared in Example 1;

[0037] Figure 3 This is a SEM image of the spinel structure high entropy ceramic aerogel material prepared in Example 1;

[0038] Figure 4 This is the energy spectrum of the spinel structure high entropy ceramic aerogel material prepared in Example 1;

[0039] Figure 5 This is the XRD pattern of the spinel structure high entropy ceramic aerogel material prepared in Example 1;

[0040] Figure 6 The nitrogen adsorption-desorption isotherm diagram of the spinel structure high entropy ceramic aerogel material prepared in Example 1;

[0041] Figure 7 This is the NLDFT pore size distribution diagram of the spinel structure high entropy ceramic aerogel material prepared in Example 1. DETAILED DESCRIPTION

[0042] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified.

[0043] 1. The present invention provides a new method for preparing high-entropy ceramic materials. Compared with the solid-phase reaction method, the operation method is completely different, so it overcomes the problems of complicated process, lengthy cycle, high equipment requirements, and abnormal growth of particle size during the sintering process.

[0044] 2. Compared with the sol-gel method and supercritical drying technology preparation method of the prior art, the present invention adopts six kinds of hydrated metal inorganic salts, and forms a wet gel with uniform components and stable structure by using a gel promoter and adjusting the ratio of organic solvent to deionized water; wherein, the gel promoter gradually consumes the hydrogen ions in the metal ion precursor solution through the epoxy ring-opening reaction, so that each component is uniformly polycondensed, and the ratio of organic solvent to deionized water is adjusted, and the concentration of the reactants and products involved in the dehydration condensation reaction can be controlled to adjust the rate and degree of the polycondensation reaction, so that the generated wet gel has uniform components and stable structure. It overcomes the problems of uneven components and unstable gel structure caused by different reaction rates of different types of precursors in the sol-gel reaction process in the prior art.

[0045] The technical solution of the present invention is further explained by using embodiments below, which are specifically as follows:

[0046] Example 1

[0047] A method for preparing a spinel structure high entropy ceramic aerogel material, wherein the chemical formula of the spinel structure high entropy ceramic aerogel material is (Mg 0.2 Co 0.2 Ni 0.2 Cu 0.2 Zn 0.2 )Al2O4, comprising the steps of:

[0048] (1) Preparation of metal ion precursor solution:

[0049] Weigh 0.683 g of magnesium nitrate hexahydrate (Mg(NO 3)2·6H2O), 0.776g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), 0.775g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 0.644g of copper nitrate trihydrate (Cu(NO3)2·3H2O), 0.793g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and 10.000g of aluminum nitrate hexahydrate (Al(NO3)3·6H2O) are weighed and added to the beaker;

[0050] 1.2 mL of deionized water and 12.3 mL of anhydrous ethanol were measured and added into a beaker, which was then placed on a magnetic stirrer and stirred at 300 rpm for 30 min at 20° C. to obtain a metal ion precursor solution;

[0051] Among them, the molar ratio of the five divalent hydrated metal inorganic salts n(Mg(NO 3)2 ·6H2O)∶n(Co(NO3)2·6H2O)∶n(Ni(NO3)2·6H2O)∶n(Cu(NO3)2·3H2O)∶n(Zn(NO3)2·6H2O)=1∶1∶1∶1∶1, the molar ratio of the total molar number of divalent hydrated metal inorganic salt to the trivalent hydrated metal inorganic salt is 0.5∶1, the molar ratio of deionized water to the trivalent hydrated metal inorganic salt is 2.5∶1, and the molar ratio of anhydrous ethanol to deionized water is 3.1∶1.

[0052] (2) Forming wet gel:

[0053] 10 mL of gel accelerator propylene oxide was measured and added to the metal ion precursor solution. The mixture was stirred at 25°C and 400 rpm for 5 min, and then allowed to stand at 20°C for 20 min to form a wet gel.

[0054] The ratio of the amount of propylene oxide to the total volume of deionized water and anhydrous ethanol is 10.6 mol:1L.

[0055] (3) Obtaining aerogel precursor:

[0056] S1. Add 20 mL of anhydrous ethanol to the wet gel, seal the beaker port with plastic wrap, and place it in a drying oven at 45° C. for 48 hours of aging to obtain an aged wet gel;

[0057] S2, washing the aged wet gel three times with anhydrous ethanol to fully remove the products of the propylene oxide ring-opening reaction remaining in the wet gel and replace the water medium, each time with an interval of 15 minutes, to obtain a washed wet gel;

[0058] S3. The washed wet gel is placed in a drying oven at 100° C. and dried at normal pressure for 24 hours to obtain an aerogel precursor.

[0059] (4) Forming spinel structure high entropy ceramic aerogel material:

[0060] The aerogel precursor was heat treated at a heating rate of 5°C / min, heated to 600°C and kept warm for 1 hour, and then cooled to room temperature in the furnace to obtain a spinel structure high entropy ceramic aerogel material.

[0061] The specific surface area of ​​the obtained spinel structure high entropy ceramic aerogel material is 243.0 m 2 / g, and the thermal conductivity at 600°C is 0.402W / (m·K).

[0062] Example 2

[0063] A method for preparing a spinel structure high entropy ceramic aerogel material, wherein the chemical formula of the spinel structure high entropy ceramic aerogel material is (Mg 0.35 Co 0.1 Ni 0.35 Cu 0.1 Zn 0.1 )Al2O4, comprising the steps of:

[0064] (1) Preparation of metal ion precursor solution:

[0065] Weigh 1.169 g of magnesium nitrate hexahydrate (Mg(NO 3)2 ·6H2O), 0.388g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), 1.375g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 0.322g of copper nitrate trihydrate (Cu(NO3)2·3H2O), 0.397g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and 10.000g of aluminum nitrate hexahydrate (Al(NO3)3·6H2O) are weighed and added to the beaker;

[0066] 2.4 mL of deionized water and 12.3 mL of anhydrous ethanol were measured and added into a beaker, which was then placed on a magnetic stirrer and stirred at 300 rpm for 30 min at 20° C. to obtain a metal ion precursor solution;

[0067] Among them, the molar ratio of the five divalent hydrated metal inorganic salts n(Mg(NO 3)2·6H2O)∶n(Co(NO3)2·6H2O)∶n(Ni(NO3)2·6H2O)∶n(Cu(NO3)2·3H2O)∶n(Zn(NO3)2·6H2O)=3.5∶1∶3.5∶1∶1, the molar ratio of the total molar number of divalent hydrated metal inorganic salt to the trivalent hydrated metal inorganic salt is 0.5∶1, the molar ratio of deionized water to the trivalent hydrated metal inorganic salt is 5∶1, and the molar ratio of anhydrous ethanol to deionized water is 1.6∶1.

[0068] (2) Forming wet gel:

[0069] 10 mL of gel accelerator propylene oxide was measured and added to the metal ion precursor solution. The mixture was stirred at 25°C and 400 rpm for 5 min, and then allowed to stand at 20°C for 20 min to form a wet gel.

[0070] The ratio of the amount of propylene oxide to the total volume of deionized water and anhydrous ethanol is 9.7 mol:1L.

[0071] (3) Obtaining aerogel precursor:

[0072] S1. Add 25 mL of anhydrous ethanol to the wet gel, seal the beaker port with plastic wrap, and place it in a drying oven at 50° C. for 42 hours of aging to obtain an aged wet gel;

[0073] S2, washing the aged wet gel with anhydrous ethanol for 3 times, each time with an interval of 15 minutes, to obtain a washed wet gel;

[0074] S3. The washed wet gel is placed in a drying oven at 90° C. and dried at normal pressure for 30 h to obtain an aerogel precursor.

[0075] (4) Forming spinel structure high entropy ceramic aerogel material:

[0076] The aerogel precursor was heat treated at a heating rate of 5°C / min, heated to 800°C and kept at this temperature for 1 hour, and then cooled to room temperature in the furnace to obtain a spinel structured high entropy ceramic aerogel material.

[0077] The specific surface area of ​​the obtained spinel structure high entropy ceramic aerogel material is 85.7 m 2 / g, and the thermal conductivity is 0.629W / (m·K) at 800℃.

[0078] Example 3

[0079] A method for preparing a spinel structure high entropy ceramic aerogel material, wherein the chemical formula of the spinel structure high entropy ceramic aerogel material is (Mg 0.3 Co 0.2 Ni 0.3 Cu0.2 Zn 0.2 )Al2O4, comprising the steps of:

[0080] (1) Preparation of metal ion precursor solution:

[0081] Weigh 0.478 g of magnesium nitrate hexahydrate (Mg(NO 3)2 ·6H2O), 0.931 g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), 0.543 g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 0.733 g of copper nitrate trihydrate (Cu(NO3)2·3H2O), 0.952 g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and 10.000 g of aluminum nitrate hexahydrate (Al(NO3)3·6H2O) are mixed and added into a beaker;

[0082] 2.4 mL of deionized water and 12.3 mL of anhydrous ethanol were measured and added into a beaker, which was then placed on a magnetic stirrer and stirred at 300 rpm for 30 min at 20° C. to obtain a metal ion precursor solution;

[0083] Among them, the molar ratio of the five divalent hydrated metal inorganic salts is n(Mg(NO 3)2 ·6H2O)∶n(Co(NO3)2·6H2O)∶n(Ni(NO3)2·6H2O)∶n(Cu(NO3)2·3H2O)∶n(Zn(NO3)2·6H2O)=3∶2∶3∶2∶2, the molar ratio of the total molar number of divalent hydrated metal inorganic salt to the trivalent hydrated metal inorganic salt is 0.5∶1, the molar ratio of deionized water to the trivalent hydrated metal inorganic salt is 5∶1, and the molar ratio of anhydrous ethanol to deionized water is 1.6∶1.

[0084] (2) Forming wet gel:

[0085] 10 mL of gel accelerator propylene oxide was measured and added to the metal ion precursor solution. The mixture was stirred at 20°C and 400 rpm for 5 min, and then allowed to stand at 20°C for 25 min to form a wet gel.

[0086] The ratio of the amount of propylene oxide to the total volume of deionized water and anhydrous ethanol is 9.7 mol:1L.

[0087] (3) Obtaining aerogel precursor:

[0088] S1. Add 25 mL of anhydrous ethanol to the wet gel, seal the beaker port with plastic wrap, and place it in a drying oven at 60° C. for 30 hours of aging to obtain an aged wet gel;

[0089] S2, washing the aged wet gel with anhydrous ethanol for 3 times, each time with an interval of 15 minutes, to obtain a washed wet gel;

[0090] S3. The washed wet gel is placed in a drying oven at 120° C. and dried at normal pressure for 20 h to obtain an aerogel precursor.

[0091] (4) Forming spinel structure high entropy ceramic aerogel material:

[0092] The aerogel precursor was heat treated at a heating rate of 5°C / min, heated to 800°C and kept at this temperature for 1 hour, and then cooled to room temperature in the furnace to obtain a spinel structured high entropy ceramic aerogel material.

[0093] The specific surface area of ​​the obtained spinel structure high entropy ceramic aerogel material is 30.7 m 2 / g, and the thermal conductivity at 800°C is 0.344W / (m·K).

[0094] Example 4

[0095] A method for preparing a spinel structure high entropy ceramic aerogel material, wherein the chemical formula of the spinel structure high entropy ceramic aerogel material is (Mg 0.2 Co 0.2 Ni 0.2 Cu 0.2 Zn 0.2 )Al2O4, comprising the steps of:

[0096] (1) Preparation of metal ion precursor solution:

[0097] Weigh 0.683 g of magnesium nitrate hexahydrate (Mg(NO 3)2 ·6H2O), 0.776g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), 0.775g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 0.644g of copper nitrate trihydrate (Cu(NO3)2·3H2O), 0.793g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and 10.000g of aluminum nitrate hexahydrate (Al(NO3)3·6H2O) are weighed and added to the beaker;

[0098] 1.2 mL of deionized water and 12.3 mL of anhydrous ethanol were measured and added into a beaker, which was then placed on a magnetic stirrer and stirred at 300 rpm for 30 min at 20° C. to obtain a metal ion precursor solution;

[0099] Among them, the molar ratio of the five divalent hydrated metal inorganic salts n(Mg(NO 3)2·6H2O)∶n(Co(NO3)2·6H2O)∶n(Ni(NO3)2·6H2O)∶n(Cu(NO3)2·3H2O)∶n(Zn(NO3)2·6H2O)=1∶1∶1∶1∶1, the molar ratio of the total molar number of divalent hydrated metal inorganic salt to the trivalent hydrated metal inorganic salt is 0.5∶1, the molar ratio of deionized water to the trivalent hydrated metal inorganic salt is 5∶1, and the molar ratio of anhydrous ethanol to deionized water is 1.6∶1.

[0100] (2) Forming wet gel:

[0101] 10 mL of gel accelerator propylene oxide was measured and added to the metal ion precursor solution. The mixture was stirred at 20°C and 400 rpm for 5 min, and then allowed to stand at 20°C for 25 min to form a wet gel.

[0102] The ratio of the amount of propylene oxide to the total volume of deionized water and anhydrous ethanol is 9.7 mol:1L.

[0103] (3) Obtaining aerogel precursor:

[0104] S1. Add 25 mL of anhydrous ethanol to the wet gel, seal the beaker port with plastic wrap, and place it in a drying oven at 45° C. for 48 hours of aging to obtain an aged wet gel;

[0105] S2, washing the aged wet gel with anhydrous ethanol for 3 times, each time with an interval of 15 minutes, to obtain a washed wet gel;

[0106] S3. The washed wet gel is placed in a drying oven at 80° C. and dried at normal pressure for 45 h to obtain an aerogel precursor.

[0107] (4) Forming spinel structure high entropy ceramic aerogel material:

[0108] The aerogel precursor was heat treated at a heating rate of 5°C / min, heated to 800°C and kept at this temperature for 1 hour, and then cooled to room temperature in the furnace to obtain a spinel structure high entropy ceramic aerogel material.

[0109] The specific surface area of ​​the obtained spinel structure high entropy ceramic aerogel material is 29.2 m 2 / g, and the thermal conductivity is 0.427W / (m·K) at 800℃.

[0110] Example 5

[0111] A method for preparing a spinel structure high entropy ceramic aerogel material, wherein the chemical formula of the spinel structure high entropy ceramic aerogel material is (Mg 0.2 Co 0.2 Ni 0.2 Cu0.2 Zn 0.2 )Al2O4, comprising the steps of:

[0112] (1) Preparation of metal ion precursor solution:

[0113] Weigh 0.683 g of magnesium nitrate hexahydrate (Mg(NO 3)2 ·6H2O), 0.776g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), 0.775g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 0.644g of copper nitrate trihydrate (Cu(NO3)2·3H2O), 0.793g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and 10.000g of aluminum nitrate hexahydrate (Al(NO3)3·6H2O) are weighed and added to the beaker;

[0114] 1.2 mL of deionized water and 12.3 mL of anhydrous ethanol were measured and added into a beaker, which was then placed on a magnetic stirrer and stirred at 300 rpm for 30 min at 20° C. to obtain a metal ion precursor solution;

[0115] Among them, the molar ratio of the five divalent hydrated metal inorganic salts is n(Mg(NO 3)2 ·6H2O)∶n(Co(NO3)2·6H2O)∶n(Ni(NO3)2·6H2O)∶n(Cu(NO3)2·3H2O)∶n(Zn(NO3)2·6H2O)=1∶1∶1∶1∶1, the molar ratio of the total molar number of divalent hydrated metal inorganic salt to the trivalent hydrated metal inorganic salt is 0.5∶1, the molar ratio of deionized water to trivalent hydrated metal inorganic salt is 2.5∶1, and the molar ratio of anhydrous ethanol to deionized water is 3.1∶1.

[0116] (2) Forming wet gel:

[0117] 10 mL of gel accelerator propylene oxide was measured and added to the metal ion precursor solution. The mixture was stirred at 20°C and 400 rpm for 5 min, and then allowed to stand at 20°C for 15 min to form a wet gel.

[0118] The ratio of the amount of propylene oxide to the total volume of deionized water and anhydrous ethanol is 10.6 mol:1L.

[0119] (3) Obtaining aerogel precursor:

[0120] S1. Add 20 mL of anhydrous ethanol to the wet gel, seal the beaker port with plastic wrap, and place it in a drying oven at 55° C. for 40 hours of aging to obtain an aged wet gel;

[0121] S2. Wash the aged wet gel three times with anhydrous ethanol, each time with an interval of 15 minutes, to obtain a washed wet gel;

[0122] S3. The washed wet gel is placed in a drying oven at 120° C. and dried at normal pressure for 20 h to obtain an aerogel precursor.

[0123] (4) Forming spinel structure high entropy ceramic aerogel material:

[0124] The aerogel precursor was heat treated at a heating rate of 5°C / min, heated to 800°C and kept at this temperature for 1 hour, and then cooled to room temperature in the furnace to obtain a spinel structured high entropy ceramic aerogel material.

[0125] The specific surface area of ​​the obtained spinel structure high entropy ceramic aerogel material is 79.1m 2 / g, and the thermal conductivity at 800°C is 0.426W / (m·K).

[0126] Example 6

[0127] A method for preparing a spinel structure high entropy ceramic aerogel material, wherein the chemical formula of the spinel structure high entropy ceramic aerogel material is (Mg 0.2 Co 0.2 Ni 0.2 Cu 0.2 Zn 0.2 )Al2O4, comprising the steps of:

[0128] (1) Preparation of metal ion precursor solution:

[0129] Weigh 0.683 g of magnesium nitrate hexahydrate (Mg(NO 3)2 ·6H2O), 0.776g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), 0.775g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 0.644g of copper nitrate trihydrate (Cu(NO3)2·3H2O), 0.793g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and 10.000g of aluminum nitrate hexahydrate (Al(NO3)3·6H2O) are weighed and added to the beaker;

[0130] 1.2 mL of deionized water and 12.3 mL of anhydrous ethanol were measured and added into a beaker, which was then placed on a magnetic stirrer and stirred at 300 rpm for 30 min at 20° C. to obtain a metal ion precursor solution;

[0131] Among them, the molar ratio of the five divalent hydrated metal inorganic salts n(Mg(NO 3)2·6H2O)∶n(Co(NO3)2·6H2O)∶n(Ni(NO3)2·6H2O)∶n(Cu(NO3)2·3H2O)∶n(Zn(NO3)2·6H2O)=1∶1∶1∶1∶1, the molar ratio of the total molar number of divalent hydrated metal inorganic salt to the trivalent hydrated metal inorganic salt is 0.5∶1, the molar ratio of deionized water to trivalent hydrated metal inorganic salt is 10∶1, and the molar ratio of anhydrous ethanol to deionized water is 0.78∶1.

[0132] (2) Forming wet gel:

[0133] 10 mL of gel accelerator propylene oxide was measured and added to the metal ion precursor solution. The mixture was stirred at 230 °C and 400 rpm for 5 min and then allowed to stand at 20 °C for 20 min to form a wet gel.

[0134] The ratio of the amount of propylene oxide to the total volume of deionized water and anhydrous ethanol is 8.3 mol:1L.

[0135] (3) Obtaining aerogel precursor:

[0136] S1. Add 28 mL of anhydrous ethanol to the wet gel, seal the beaker port with plastic wrap, and place it in a drying oven at 60° C. for 30 hours of aging to obtain an aged wet gel;

[0137] S2, washing the aged wet gel with anhydrous ethanol for 3 times, each time with an interval of 15 minutes, to obtain a washed wet gel;

[0138] S3. The washed wet gel is placed in a drying oven at 100° C. and dried at normal pressure for 24 hours to obtain an aerogel precursor.

[0139] (4) Forming spinel structure high entropy ceramic aerogel material:

[0140] The aerogel precursor was heat treated at a heating rate of 5°C / min, heated to 800°C and kept at this temperature for 1 hour, and then cooled to room temperature in the furnace to obtain a spinel structured high entropy ceramic aerogel material.

[0141] The specific surface area of ​​the obtained spinel structure high entropy ceramic aerogel material is 56.3 m 2 / g, and the thermal conductivity at 800°C is 0.475W / (m·K).

[0142] Example 7

[0143] A method for preparing a spinel structure high entropy ceramic aerogel material, wherein the chemical formula of the spinel structure high entropy ceramic aerogel material is (Mg 0.2 Co 0.2 Ni 0.2 Cu0.2 Zn 0.2 )Al2O4, comprising the steps of:

[0144] (1) Preparation of metal ion precursor solution:

[0145] Weigh 0.683 g of magnesium nitrate hexahydrate (Mg(NO 3)2 ·6H2O), 0.776g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), 0.775g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 0.644g of copper nitrate trihydrate (Cu(NO3)2·3H2O), 0.793g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and 10.000g of aluminum nitrate hexahydrate (Al(NO3)3·6H2O) are weighed and added to the beaker;

[0146] 1.2 mL of deionized water and 12.3 mL of anhydrous ethanol were measured and added into a beaker, which was then placed on a magnetic stirrer and stirred at 300 rpm for 30 min at 20° C. to obtain a metal ion precursor solution;

[0147] Among them, the molar ratio of the five divalent hydrated metal inorganic salts is n(Mg(NO 3)2 ·6H2O)∶n(Co(NO3)2·6H2O)∶n(Ni(NO3)2·6H2O)∶n(Cu(NO3)2·3H2O)∶n(Zn(NO3)2·6H2O)=1∶1∶1∶1∶1, the molar ratio of the total molar number of divalent hydrated metal inorganic salt to the trivalent hydrated metal inorganic salt is 0.5∶1, the molar ratio of deionized water to the trivalent hydrated metal inorganic salt is 2.5∶1, and the molar ratio of anhydrous ethanol to deionized water is 3.1∶1.

[0148] (2) Forming wet gel:

[0149] 10 mL of gel accelerator propylene oxide was measured and added to the metal ion precursor solution. The mixture was stirred at 30°C and 400 rpm for 5 min, and then allowed to stand at 20°C for 25 min to form a wet gel.

[0150] The ratio of the amount of propylene oxide to the total volume of deionized water and anhydrous ethanol is 8.5 mol:1L.

[0151] (3) Obtaining aerogel precursor:

[0152] S1. Add 23 mL of anhydrous ethanol to the wet gel, seal the beaker port with plastic wrap, and place it in a drying oven at 50° C. for 42 hours of aging to obtain an aged wet gel;

[0153] S2, washing the aged wet gel with anhydrous ethanol for 3 times, each time with an interval of 15 minutes, to obtain a washed wet gel;

[0154] S3. The washed wet gel is placed in a drying oven at 90° C. and dried at normal pressure for 30 h to obtain an aerogel precursor.

[0155] (4) Forming spinel structure high entropy ceramic aerogel material:

[0156] The aerogel precursor was heat treated at a heating rate of 5°C / min, heated to 800°C and kept at this temperature for 1 hour, and then cooled to room temperature in the furnace to obtain a spinel structured high entropy ceramic aerogel material.

[0157] The specific surface area of ​​the obtained spinel structure high entropy ceramic aerogel material is 43.3 m 2 / g, and the thermal conductivity at 800°C is 0.452W / (m·K).

[0158] Example 8

[0159] A method for preparing a spinel structure high entropy ceramic aerogel material, wherein the chemical formula of the spinel structure high entropy ceramic aerogel material is (Mg 0.05 Co 0.35 Ni 0.05 Cu 0.35 Zn 0.2 )Fe2O4, comprising the following steps:

[0160] (1) Preparation of metal ion precursor solution:

[0161] Weigh magnesium nitrate hexahydrate (Mg(NO 3)2 ·6H2O), cobalt nitrate hexahydrate (Co(NO3)2·6H2O), nickel nitrate hexahydrate (Ni(NO3)2·6H2O), copper nitrate trihydrate (Cu(NO3)2·3H2O), zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and trivalent hydrated metal inorganic salts of ferric chloride hexahydrate (FeCl3·6H2O), mixed and added to the beaker;

[0162] Deionized water and anhydrous ethanol were measured and added into a beaker, which was then placed on a magnetic stirrer and stirred at 40° C. and 500 rpm for 60 min to obtain a metal ion precursor solution;

[0163] Among them, the molar ratio of the five divalent hydrated metal inorganic salts is n(Mg(NO 3)2·6H2O)∶n(Co(NO3)2·6H2O)∶n(Ni(NO3)2·6H2O)∶n(Cu(NO3)2·3H2O)∶n(Zn(NO3)2·6H2O)=0.05∶0.35∶0.05∶0.35∶0.2, the molar ratio of the total molar number of divalent hydrated metal inorganic salt to the trivalent hydrated metal inorganic salt is 0.5∶1, the molar ratio of deionized water to the trivalent hydrated metal inorganic salt is 25∶1, and the molar ratio of anhydrous ethanol to deionized water is 4∶1.

[0164] (2) Forming wet gel:

[0165] The gel accelerator epoxybutene was measured and added to the metal ion precursor solution, and the mixture was stirred continuously for 10 min at 20°C and 600 rpm, and then allowed to stand at 60°C for 20 min to form a wet gel;

[0166] The ratio of the amount of epoxybutene substance to the total volume of deionized water and anhydrous ethanol is 24 mol: 1L.

[0167] (3) Obtaining aerogel precursor:

[0168] S1. Add anhydrous ethanol to the wet gel, seal the beaker port with plastic wrap, and place it in a drying oven at 40° C. for 72 hours of aging to obtain an aged wet gel;

[0169] S2, washing the aged wet gel with anhydrous ethanol for 3 times, each time with an interval of 10 minutes, to obtain a washed wet gel;

[0170] S3. The washed wet gel is placed in a drying oven at 80° C. and dried at normal pressure for 48 hours to obtain an aerogel precursor.

[0171] (4) Forming spinel structure high entropy ceramic aerogel material:

[0172] The aerogel precursor was heat treated at a heating rate of 5°C / min, heated to 1000°C and kept warm for 1.5 hours, and then cooled to room temperature in the furnace to obtain a spinel structured high entropy ceramic aerogel material.

[0173] Example 9

[0174] A method for preparing a spinel structure high entropy ceramic aerogel material, wherein the chemical formula of the spinel structure high entropy ceramic aerogel material is (Mg 0.2 Co 0.35 Ni 0.05 Cu 0.05 Zn 0.35 )Fe2O4, comprising the following steps:

[0175] (1) Preparation of metal ion precursor solution:

[0176] Weigh magnesium nitrate hexahydrate (Mg(NO 3)2 ·6H2O), cobalt nitrate hexahydrate (Co(NO3)2·6H2O), nickel nitrate hexahydrate (Ni(NO3)2·6H2O), copper nitrate trihydrate (Cu(NO3)2·3H2O), zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and trivalent hydrated metal inorganic salts of ferric chloride hexahydrate (FeCl3·6H2O), mixed and added to the beaker;

[0177] Deionized water and anhydrous ethanol were measured and added into a beaker, which was then placed on a magnetic stirrer and stirred at 50° C. and 600 rpm for 5 min to obtain a metal ion precursor solution;

[0178] Among them, the molar ratio of the five divalent hydrated metal inorganic salts is n(Mg(NO 3)2 ·6H2O)∶n(Co(NO3)2·6H2O)∶n(Ni(NO3)2·6H2O)∶n(Cu(NO3)2·3H2O)∶n(Zn(NO3)2·6H2O)=0.2∶0.35∶0.05∶0.05∶0.35, the molar ratio of the total molar number of divalent hydrated metal inorganic salt to the trivalent hydrated metal inorganic salt is 0.5∶1, the molar ratio of deionized water to the trivalent hydrated metal inorganic salt is 2∶1, and the molar ratio of anhydrous ethanol to deionized water is 0.4∶1.

[0179] (2) Forming wet gel:

[0180] The gel accelerator epibromopropane was measured and added to the metal ion precursor solution, and the mixture was stirred continuously for 20 minutes at 50°C and 300 rpm, and then allowed to stand at 40°C for 20 minutes to form a wet gel;

[0181] The ratio of the amount of propylene oxide to the total volume of deionized water and anhydrous ethanol is 1.7 mol:1L.

[0182] (3) Obtaining aerogel precursor:

[0183] S1. Add n-butanol to the wet gel, seal the beaker port with plastic wrap, and place it in a drying oven at 65° C. for 24 hours to obtain an aged wet gel;

[0184] S2, washing the aged wet gel three times with anhydrous ethanol, each time with an interval of 30 minutes, to obtain a washed wet gel;

[0185] S3. The washed wet gel is placed in a drying oven at 150° C. and dried at normal pressure for 24 h to obtain an aerogel precursor.

[0186] (4) Forming spinel structure high entropy ceramic aerogel material:

[0187] The aerogel precursor was heat treated at a heating rate of 5°C / min, heated to 1200°C and kept warm for 1 hour, and then cooled to room temperature in the furnace to obtain a spinel structured high entropy ceramic aerogel material.

[0188] Examples 1-9 of the present invention all produce spinel structure high entropy ceramic aerogel materials with high specific surface area and low high temperature thermal conductivity. The spinel structure high entropy ceramic aerogel material of Example 1 is used as an example for research. The specific research method and results are as follows:

[0189] Figure 1 This is a real picture of wet gel. Figure 1 The results showed that the prepared wet gel was in block shape and had a certain structural stability.

[0190] Figure 2 This is a physical picture of spinel structure high entropy ceramic aerogel. Figure 2 The results show that the prepared spinel structure high entropy ceramic aerogel material is brown-black and relatively uniform.

[0191] Figure 3 For SEM images, Figure 3 The results show that the prepared spinel structured high entropy ceramic aerogel material has a uniform network skeleton structure formed by nanoparticles.

[0192] Figure 4 is the energy spectrum, Figure 4 The results show that the elements of the prepared spinel structure high entropy ceramic aerogel material are evenly distributed and the components are uniform.

[0193] Figure 5 is the XRD pattern, Figure 5 The results show that the prepared spinel structured high entropy ceramic aerogel material presents a spinel single-phase solid solution crystal structure.

[0194] Figure 6 is the nitrogen adsorption-desorption isotherm, Figure 6 The results show that the prepared spinel structured high entropy ceramic aerogel material has the isotherms and hysteresis loop types of typical mesoporous materials.

[0195] Figure 7 is the NLDFT pore size distribution diagram, Figure 7 The results show that the prepared spinel structure high entropy ceramic aerogel material has nanoscale pores, and the pore size is mainly distributed in the range of 10 to 40 nm.

[0196] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, they are also intended to be included.

Claims

1. A spinel structure high entropy ceramic aerogel material, It is characterized in that The expression of the spinel structure high entropy ceramic aerogel material is (Mg x1 Co x2 Ni x3 Cu x4 Zn x5 )M 2 O 4 , x 1 、x 2 、x 3 、x 4 and x 5 are the ratios of the number of atoms, x 1 +x 2 +x 3 +x 4 +x 5 =1,0.05≤x 1 ≤0.35, 0.05≤x 2 ≤0.35, 0.05≤x 3 ≤0.35, 0.05≤x 4 ≤0.35, 0.05≤x 5 ≤0.35, M is one of Al, Cr, Mn and Fe.

2. A method for preparing the spinel structure high entropy ceramic aerogel material according to claim 1, It is characterized in that The steps include: Weighing divalent hydrated inorganic salts of Mg, Co, Ni, Cu and Zn respectively, weighing one of trivalent hydrated inorganic salts of Al, Cr, Mn and Fe, and mixing the five divalent hydrated inorganic salts with one trivalent hydrated inorganic salt to obtain a mixed inorganic salt; Adding a solvent to the mixed inorganic salt and dispersing the mixture uniformly to obtain a metal ion precursor solution; Adding a gel accelerator, which is an epoxy compound, to the metal ion precursor solution, and mixing them evenly, and standing them until a gel transition occurs to obtain a wet gel; The wet gel is subjected to an aging treatment, and then washed and dried to obtain an aerogel precursor; The aerogel precursor is heat-treated to obtain a spinel structure high entropy ceramic aerogel material.

3. The method for preparing the spinel structure high entropy ceramic aerogel material according to claim 2, It is characterized in that The molar ratio of five divalent hydrated inorganic salts of Mg, Co, Ni, Cu and Zn is 1-7:1-7:1-7:1-7:1-7.

4. The method for preparing the spinel structure high entropy ceramic aerogel material according to claim 2, It is characterized in that The ratio of the total molar amount of the five divalent hydrated inorganic salts to the molar amount of the one trivalent hydrated inorganic salt is 0.5:

1.

5. The method for preparing the spinel structure high entropy ceramic aerogel material according to claim 2, It is characterized in that The solvent consists of deionized water and an organic solvent, the organic solvent is selected from methanol, ethanol, isopropanol, n-butanol, n-pentane, acetonitrile or dimethylformamide, and the molar ratio of the organic solvent to the deionized water is 0.4-4:

1.

6. The method for preparing the spinel structure high entropy ceramic aerogel material according to claim 5, It is characterized in that The molar ratio of deionized water to trivalent hydrated inorganic salt is 2-25:

1.

7. The method for preparing the spinel structure high entropy ceramic aerogel material according to claim 2, It is characterized in that The volume ratio of the gel accelerator substance to the solvent is 1.7 to 24 mol:1L.

8. The method for preparing the spinel structure high entropy ceramic aerogel material according to claim 2, It is characterized in that The aging treatment method is: the wet gel is mixed with the aging agent, sealed, and aged at 40-65°C for 24-72h; The aging agent is selected from one or more of methanol, ethanol, isopropanol, n-butanol, n-pentane, acetonitrile and dimethylformamide.

9. The method for preparing the spinel structure high entropy ceramic aerogel material according to claim 2, It is characterized in that The heat treatment method is: keep warm at 600-1200°C in air atmosphere for 1-2 hours.

10. Use of the spinel structure high entropy ceramic aerogel material according to claim 1 in preparing thermal insulation materials or high temperature resistant materials.

Citation Information

Patent Citations

  • Low-thermal-conductivity infrared emission material as well as preparation method and application thereof

    CN114956802A

  • Preparation method of (LaCeSmEuNd) 2Zr2O7 high-entropy oxide ceramic aerogel

    CN115141030A

  • Methods of preparing aerogels and aerogel slurries and aerogels and slurries prepared thereby

    GB202307406D0

  • Method for preparing bulk c-aln composite aerogel with high strength and high temperature resistance

    US20150108389A1

Cited By

  • Cationic anti-stable aluminate high-entropy ceramic and wide-temperature-range preparation method

    CN122036340A