High-resilience sponge material and preparation method thereof
The sponge material was solved by using raw materials such as ammonium polyphosphate, alkali lignin and diphenylmethane diisocyanate in sponge materials, and combined with polyester polyol block prepolymers. The problem of insufficient resilience and flame retardancy has achieved the preparation of sponge materials with high resilience and excellent flame retardancy.
Patent Information
- Application Number
- CN202410977229.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-19
AI Technical Summary
Existing sponge materials have shortcomings in terms of resilience, durability and flame retardancy, making it difficult to meet the needs of modern life.
The expanded flame retardant components are prepared by ammonium polyphosphate, alkali lignin and diphenylmethane diisocyanate, and the homemade polyurethane is prepared by foaming process. Highly resilient sponge material improves flame retardant performance by combining the expansion-type and halogen-free reactive flame retardant components.
It achieves high resilience and excellent flame retardant effect, improves the durability and flame retardant performance of sponge materials, and is suitable for furniture, car seats and other applications.
Smart Images

Figure BDA0004954930440000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sponge materials, and in particular to a high-resilience sponge material and a preparation method thereof. Background Art
[0002] With the advancement of science and technology and the improvement of people's requirements for the quality of life, the demand for various material properties is also increasing, especially in the fields of daily necessities such as furniture, car seats, mattresses, etc., the requirements for the performance of materials such as resilience, comfort, and durability are particularly strict. Sponge materials are widely used in these fields due to their good elasticity and comfort. However, traditional sponge materials have many deficiencies in terms of resilience and durability, and it is difficult to meet the needs of modern life. Therefore, the development of a highly resilient, durable and comfortable sponge material and its preparation method is of great significance to improving the quality of related products and user experience.
[0003] At present, the sponge materials on the market are mainly produced based on polyurethane foaming technology. By adjusting the raw material ratio and process parameters, sponge products with different properties can be obtained. However, these products generally have the following problems: insufficient resilience, poor durability, poor environmental protection and poor flame retardancy. In order to solve the above problems, it is necessary to improve the existing sponge material preparation method. Summary of the invention
[0004] Technical issues solved
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a high-resilience sponge material and a preparation method thereof, which can effectively solve the problems of insufficient resilience and poor flame retardancy of the sponge material in the prior art.
[0006] Technical Solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A method for preparing a high resilience sponge material, the preparation method comprising the following steps:
[0009] S1, using ammonium polyphosphate, alkali lignin and diphenylmethane diisocyanate as raw materials to prepare an intumescent flame retardant component, and using 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and as raw materials to prepare a halogen-free reactive flame retardant component;
[0010] S2, using polyester polyol block prepolymer and 1,4-butylene diisocyanate as raw materials to prepare self-made polyurethane, then using anhydrous ethanol as a precipitation washing liquid to precipitate and purify the self-made polyurethane, and the obtained precipitate is recorded as solid polyurethane after drying;
[0011] S3. Weigh 30-35g of solid polyurethane, 18-20g of polyethylene glycol 4000, 26-30g of dioxane and 5-6g of toluene diisocyanate, mix and stir, stir and react at 60°C for 20min, then pour into a mold for foaming, after foaming, place in a freeze dryer at 20°C for freezing at normal pressure for 3h, then place in a vacuum dryer at 25°C for 12h, and the obtained sponge material is a high resilience sponge material.
[0012] Furthermore, in S1, the preparation steps of the intumescent flame retardant component are:
[0013] Step 1, weigh 45g of ammonium polyphosphate and disperse it in a flask filled with 250mL of ethyl acetate, add 10g of diphenylmethane diisocyanate, heat it in a water bath to 50°C, and stir and mix for 1h, then add 5g of alkali lignin, heat it in a water bath to 60°C, and react at this temperature for 5h, the result is recorded as the reaction component;
[0014] Step 2: Filter the reaction components to remove the filtrate, then wash with ethyl acetate three times, dry and grind through an 80-mesh sieve to obtain an intumescent flame retardant component.
[0015] Furthermore, in step one, the stirring speed of the stirring mixture is 300 r / min, and in step two, the drying method is to place the mixture in an oven at 80° C. and dry it for 24 hours.
[0016] Furthermore, in S1, the preparation steps of the halogen-free reactive flame retardant component are:
[0017] Step A, weigh 10g 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 200mL xylene into a flask, heat to 90°C under nitrogen protection, stir to dissolve and then add 20mL formaldehyde dropwise, react at the original temperature for 6h after the addition is completed, and the result is recorded as the reaction system;
[0018] Step B, cooling the reaction system to room temperature and filtering to obtain a solid product, washing it with anhydrous ethanol for three times, drying it and grinding it through a 200-mesh sieve to obtain a halogen-free reactive flame retardant component.
[0019] Furthermore, in step A, the stirring and dissolving method is stirring at a stirring speed of 200 r / min for 10 minutes, the dripping rate in step A is 1 drop / s, and in step B, the drying method is placing in an oven at 65° C. and drying for 5 hours.
[0020] Furthermore, in S2, the preparation steps of the polyester polyol block prepolymer are:
[0021] Step 1, weigh 30g polyethylene glycol, 8g D, L-lactide, 10g trimethylene carbonate and 0.1g stannous octoate into a flask, mix well, evacuate and replace with nitrogen three times, then heat to 130°C and keep warm for 6h, the result is recorded as the block prepolymer component;
[0022] Step 2: Pour 200 mL of dichloromethane into the block prepolymer component, and then use petroleum ether as a precipitation washing liquid to perform precipitation purification treatment to obtain a polyester polyol block prepolymer wet material, and the obtained polyester polyol block prepolymer is obtained after drying treatment.
[0023] Furthermore, in step 1, the method for uniform mixing is stirring at a stirring speed of 150 r / min for 10 minutes, and in step 2, the method for drying is placing in a vacuum drying oven at 40° C. for 12 hours.
[0024] Furthermore, in S2, the preparation method of the homemade polyurethane is:
[0025] 1) Weigh 70g of polyester polyol block prepolymer and 30g of 1,4-butanediisocyanate into a reaction kettle, add 1g of N,N′-dimethylformamide, evacuate and replace with nitrogen three times, heat to 80°C and react at constant temperature for 4h, the result is recorded as reaction mixture;
[0026] 2) Add 0.1 g of stannous octoate and 20 g of 1,4-butanediol to the reaction mixture, evacuate the mixture again and replace it with nitrogen three times, and then react at a constant temperature of 80° C. for 6 h to obtain the self-made polyurethane.
[0027] Furthermore, in S2, the drying method is to place the mixture in a vacuum drying oven at 60°C for 10 hours, and in S3, the mixing and stirring method is to stir the mixture at a stirring speed of 300 r / min for 10 minutes, and the foaming time is 3-5 minutes.
[0028] A high resilience sponge material is prepared by a high resilience sponge material preparation method.
[0029] Beneficial Effects
[0030] The present invention provides a high resilience sponge material and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The intumescent flame retardant component prepared by the present invention with ammonium polyphosphate, alkali lignin and diphenylmethane diisocyanate as raw materials, alkali lignin as a natural polymer compound, adding it can increase the stability of the carbonized layer and further improve the flame retardant effect, diphenylmethane diisocyanate as one of the raw materials for preparing polyurethane sponge, the benzene ring in its structure can enhance the stability of the carbonized layer, thereby improving the flame retardant performance; secondly, the intumescent flame retardant component can be matched with the halogen-free reactive flame retardant component, and it is added to the preparation of polyurethane sponge, the intumescent flame retardant component mainly isolates oxygen and heat by forming a carbonized layer, and the halogen-free reactive flame retardant component may achieve flame retardancy by capturing free radicals in the flame, generating non-flammable gas, etc. The mutual matching of the two flame retardant components can give full play to their respective advantages and achieve better flame retardant effect.
[0032] 2. The present invention uses polyester polyol block prepolymer and 1,4-butylene diisocyanate as raw materials to prepare self-made polyurethane, and then uses the self-made polyurethane as raw material to prepare sponge material through foaming. The polyester polyol block prepolymer is a polymer compound, and its molecular structure contains multiple hydroxyl functional groups, which can react with 1,4-butylene diisocyanate to generate polyurethane. This reaction can form a cross-linked structure between polymer chains, so that the polyurethane sponge material has higher elasticity and resilience. After being compressed by external force, the polyurethane sponge material can quickly recover to its original shape and volume, showing excellent resilience. This high resilience enables the polyurethane sponge material to provide better support and comfort in applications such as seat cushions and mattresses. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The present invention will be further described below in conjunction with the embodiments.
[0035] Example 1
[0036] A method for preparing a high resilience sponge material in this embodiment comprises the following steps:
[0037] S1, using ammonium polyphosphate, alkali lignin and diphenylmethane diisocyanate as raw materials to prepare an intumescent flame retardant component, and using 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and as raw materials to prepare a halogen-free reactive flame retardant component;
[0038] S2, using polyester polyol block prepolymer and 1,4-butylene diisocyanate as raw materials to prepare self-made polyurethane, then using anhydrous ethanol as a precipitation washing liquid to precipitate and purify the self-made polyurethane, and the obtained precipitate is recorded as solid polyurethane after drying;
[0039] S3. Weigh 30g of solid polyurethane, 18g of polyethylene glycol 4000, 26g of dioxane and 5g of toluene diisocyanate, mix and stir, react at 60°C for 20min, then pour into a mold for foaming, place in a freeze dryer at 20°C for freezing at normal pressure for 3h, then place in a vacuum dryer at 25°C for 12h, and the result is a high resilience sponge material.
[0040] In S1, the preparation steps of the intumescent flame retardant component are:
[0041] Step 1, weigh 45g of ammonium polyphosphate and disperse it in a flask filled with 250mL of ethyl acetate, add 10g of diphenylmethane diisocyanate, heat it in a water bath to 50°C, and stir and mix for 1h, then add 5g of alkali lignin, heat it in a water bath to 60°C, and react at this temperature for 5h, the result is recorded as the reaction component;
[0042] Step 2: Filter the reaction components to remove the filtrate, then wash with ethyl acetate three times, dry and grind through an 80-mesh sieve to obtain an intumescent flame retardant component.
[0043] In step one, the stirring speed of the stirring mixture is 300 r / min, and in step two, the drying method is to place the mixture in an oven at 80° C. and dry it for 24 hours.
[0044] In S1, the preparation steps of the halogen-free reactive flame retardant component are:
[0045] Step A, weigh 10g 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 200mL xylene into a flask, heat to 90°C under nitrogen protection, stir to dissolve and then add 20mL formaldehyde dropwise, react at the original temperature for 6h after the addition is completed, and the result is recorded as the reaction system;
[0046] Step B, cooling the reaction system to room temperature and filtering to obtain a solid product, washing it with anhydrous ethanol for three times, drying it and grinding it through a 200-mesh sieve to obtain a halogen-free reactive flame retardant component.
[0047] In step A, the stirring and dissolving method is to stir at a stirring speed of 200 r / min for 10 minutes, the dripping rate in step A is 1 drop / s, and in step B, the drying method is to place in an oven at 65° C. and dry for 5 hours.
[0048] In S2, the preparation steps of the polyester polyol block prepolymer are:
[0049] Step 1, weigh 30g polyethylene glycol, 8g D, L-lactide, 10g trimethylene carbonate and 0.1g stannous octoate into a flask, mix well, evacuate and replace with nitrogen three times, then heat to 130°C and keep warm for 6h, the result is recorded as the block prepolymer component;
[0050] Step 2: Pour 200 mL of dichloromethane into the block prepolymer component, and then use petroleum ether as a precipitation washing liquid to perform precipitation purification treatment to obtain a polyester polyol block prepolymer wet material, and the obtained polyester polyol block prepolymer is obtained after drying treatment.
[0051] In step 1, the method for uniform mixing is to stir at a stirring speed of 150 r / min for 10 minutes. In step 2, the method for drying is to place in a vacuum drying oven at 40° C. and dry for 12 hours.
[0052] In S2, the preparation method of the homemade polyurethane is:
[0053] 1) Weigh 70g of polyester polyol block prepolymer and 30g of 1,4-butanediisocyanate into a reaction kettle, add 1g of N,N′-dimethylformamide, evacuate and replace with nitrogen three times, heat to 80°C and react at constant temperature for 4h, the result is recorded as reaction mixture;
[0054] 2) Add 0.1 g of stannous octoate and 20 g of 1,4-butanediol to the reaction mixture, evacuate the mixture again and replace it with nitrogen three times, and then react at a constant temperature of 80° C. for 6 h to obtain the self-made polyurethane.
[0055] In S2, the drying method is to place the mixture in a vacuum drying oven at 60°C for 10 hours. In S3, the mixing and stirring method is to stir the mixture at a stirring speed of 300 r / min for 10 minutes, and the foaming time is 3 minutes.
[0056] A high resilience sponge material is prepared by a high resilience sponge material preparation method.
[0057] Example 2
[0058] A method for preparing a high resilience sponge material in this embodiment comprises the following steps:
[0059] S1, using ammonium polyphosphate, alkali lignin and diphenylmethane diisocyanate as raw materials to prepare an intumescent flame retardant component, and using 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and as raw materials to prepare a halogen-free reactive flame retardant component;
[0060] S2, using polyester polyol block prepolymer and 1,4-butylene diisocyanate as raw materials to prepare self-made polyurethane, then using anhydrous ethanol as a precipitation washing liquid to precipitate and purify the self-made polyurethane, and the obtained precipitate is recorded as solid polyurethane after drying;
[0061] S3. Weigh 35g of solid polyurethane, 20g of polyethylene glycol 4000, 30g of dioxane and 6g of toluene diisocyanate, mix and stir, stir and react at 60°C for 20min, then pour into a mold for foaming, place in a freeze dryer at 20°C for freezing at normal pressure for 3h, then place in a vacuum dryer at 25°C for 12h, and the result is a high resilience sponge material.
[0062] In S1, the preparation steps of the intumescent flame retardant component are:
[0063] Step 1, weigh 45g of ammonium polyphosphate and disperse it in a flask filled with 250mL of ethyl acetate, add 10g of diphenylmethane diisocyanate, heat it in a water bath to 50°C, and stir and mix for 1h, then add 5g of alkali lignin, heat it in a water bath to 60°C, and react at this temperature for 5h, the result is recorded as the reaction component;
[0064] Step 2: Filter the reaction components to remove the filtrate, then wash with ethyl acetate three times, dry and grind through an 80-mesh sieve to obtain an intumescent flame retardant component.
[0065] In step one, the stirring speed of the stirring mixture is 300 r / min, and in step two, the drying method is to place the mixture in an oven at 80° C. and dry it for 24 hours.
[0066] In S1, the preparation steps of the halogen-free reactive flame retardant component are:
[0067] Step A, weigh 10g 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 200mL xylene into a flask, heat to 90°C under nitrogen protection, stir to dissolve and then add 20mL formaldehyde dropwise, react at the original temperature for 6h after the addition is completed, and the result is recorded as the reaction system;
[0068] Step B, cooling the reaction system to room temperature and filtering to obtain a solid product, washing it with anhydrous ethanol for three times, drying it and grinding it through a 200-mesh sieve to obtain a halogen-free reactive flame retardant component.
[0069] In step A, the stirring and dissolving method is to stir at a stirring speed of 200 r / min for 10 minutes, the dripping rate in step A is 1 drop / s, and in step B, the drying method is to place in an oven at 65° C. and dry for 5 hours.
[0070] In S2, the preparation steps of the polyester polyol block prepolymer are:
[0071] Step 1, weigh 30g polyethylene glycol, 8g D, L-lactide, 10g trimethylene carbonate and 0.1g stannous octoate into a flask, mix well, evacuate and replace with nitrogen three times, then heat to 130°C and keep warm for 6h, the result is recorded as the block prepolymer component;
[0072] Step 2: Pour 200 mL of dichloromethane into the block prepolymer component, and then use petroleum ether as a precipitation washing liquid to perform precipitation purification treatment to obtain a polyester polyol block prepolymer wet material, and the obtained polyester polyol block prepolymer is obtained after drying treatment.
[0073] In step 1, the method for uniform mixing is to stir at a stirring speed of 150 r / min for 10 minutes. In step 2, the method for drying is to place in a vacuum drying oven at 40° C. and dry for 12 hours.
[0074] In S2, the preparation method of the homemade polyurethane is:
[0075] 1) Weigh 70g of polyester polyol block prepolymer and 30g of 1,4-butanediisocyanate into a reaction kettle, add 1g of N,N′-dimethylformamide, evacuate and replace with nitrogen three times, heat to 80°C and react at constant temperature for 4h, the result is recorded as reaction mixture;
[0076] 2) Add 0.1 g of stannous octoate and 20 g of 1,4-butanediol to the reaction mixture, evacuate the mixture again and replace it with nitrogen three times, and then react at a constant temperature of 80° C. for 6 h to obtain the self-made polyurethane.
[0077] In S2, the drying method is to place the mixture in a vacuum drying oven at 60°C for 10 hours. In S3, the mixing and stirring method is to stir the mixture at a stirring speed of 300 r / min for 10 minutes, and the foaming time is 5 minutes.
[0078] A high resilience sponge material is prepared by a high resilience sponge material preparation method.
[0079] Example 3
[0080] A method for preparing a high resilience sponge material in this embodiment comprises the following steps:
[0081] S1, using ammonium polyphosphate, alkali lignin and diphenylmethane diisocyanate as raw materials to prepare an intumescent flame retardant component, and using 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and as raw materials to prepare a halogen-free reactive flame retardant component;
[0082] S2, using polyester polyol block prepolymer and 1,4-butylene diisocyanate as raw materials to prepare self-made polyurethane, then using anhydrous ethanol as a precipitation washing liquid to precipitate and purify the self-made polyurethane, and the obtained precipitate is recorded as solid polyurethane after drying;
[0083] S3. Weigh 33g of solid polyurethane, 19g of polyethylene glycol 4000, 28g of dioxane and 6g of toluene diisocyanate, mix and stir, stir and react at 60°C for 20min, then pour into a mold for foaming, place in a freeze dryer at 20°C for freezing at normal pressure for 3h, then place in a vacuum dryer at 25°C for 12h, and the result is a high resilience sponge material.
[0084] In S1, the preparation steps of the intumescent flame retardant component are:
[0085] Step 1, weigh 45g of ammonium polyphosphate and disperse it in a flask filled with 250mL of ethyl acetate, add 10g of diphenylmethane diisocyanate, heat it in a water bath to 50°C, and stir and mix for 1h, then add 5g of alkali lignin, heat it in a water bath to 60°C, and react at this temperature for 5h, the result is recorded as the reaction component;
[0086] Step 2: Filter the reaction components to remove the filtrate, then wash with ethyl acetate three times, dry and grind through an 80-mesh sieve to obtain an intumescent flame retardant component.
[0087] In step one, the stirring speed of the stirring mixture is 300 r / min, and in step two, the drying method is to place the mixture in an oven at 80° C. and dry it for 24 hours.
[0088] In S1, the preparation steps of the halogen-free reactive flame retardant component are:
[0089] Step A, weigh 10g 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 200mL xylene into a flask, heat to 90°C under nitrogen protection, stir to dissolve and then add 20mL formaldehyde dropwise, react at the original temperature for 6h after the addition is completed, and the result is recorded as the reaction system;
[0090] Step B, cooling the reaction system to room temperature and filtering to obtain a solid product, washing it with anhydrous ethanol for three times, drying it and grinding it through a 200-mesh sieve to obtain a halogen-free reactive flame retardant component.
[0091] In step A, the stirring and dissolving method is to stir at a stirring speed of 200 r / min for 10 minutes, the dripping rate in step A is 1 drop / s, and in step B, the drying method is to place in an oven at 65° C. and dry for 5 hours.
[0092] In S2, the preparation steps of the polyester polyol block prepolymer are:
[0093] Step 1, weigh 30g polyethylene glycol, 8g D, L-lactide, 10g trimethylene carbonate and 0.1g stannous octoate into a flask, mix well, evacuate and replace with nitrogen three times, then heat to 130°C and keep warm for 6h, the result is recorded as the block prepolymer component;
[0094] Step 2: Pour 200 mL of dichloromethane into the block prepolymer component, and then use petroleum ether as a precipitation washing liquid to perform precipitation purification treatment to obtain a polyester polyol block prepolymer wet material, and the obtained polyester polyol block prepolymer is obtained after drying treatment.
[0095] In step 1, the method for uniform mixing is to stir at a stirring speed of 150 r / min for 10 minutes. In step 2, the method for drying is to place in a vacuum drying oven at 40° C. and dry for 12 hours.
[0096] In S2, the preparation method of the homemade polyurethane is:
[0097] 1) Weigh 70g of polyester polyol block prepolymer and 30g of 1,4-butanediisocyanate into a reaction kettle, add 1g of N,N′-dimethylformamide, evacuate and replace with nitrogen three times, heat to 80°C and react at constant temperature for 4h, the result is recorded as reaction mixture;
[0098] 2) Add 0.1 g of stannous octoate and 20 g of 1,4-butanediol to the reaction mixture, evacuate the mixture again and replace it with nitrogen three times, and then react at a constant temperature of 80° C. for 6 h to obtain the self-made polyurethane.
[0099] In S2, the drying method is to place the mixture in a vacuum drying oven at 60°C for 10 hours. In S3, the mixing and stirring method is to stir the mixture at a stirring speed of 300 r / min for 10 minutes, and the foaming time is 4 minutes.
[0100] A high resilience sponge material is prepared by a high resilience sponge material preparation method.
[0101] Comparative Example 1
[0102] The high resilience sponge material and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 1, the intumescent flame retardant component in Example 1 is replaced with a halogen-free reactive flame retardant component.
[0103] Comparative Example 2
[0104] The high resilience sponge material and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 2, the halogen-free reactive flame retardant component in Example 1 is replaced with an intumescent flame retardant component.
[0105] Performance Testing
[0106] The high resilience sponge materials in Examples 1-3 and Comparative Examples 1-2 are marked as Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2, respectively. The performance of Examples 1-3 and Comparative Examples 1-2 is then tested, and the obtained data is recorded in the following table:
[0107]
[0108] The data in the above table show that the high resilience sponge materials prepared in Examples 1-3 have high compressive strength and tensile strength, and have high resilience. Compared with Comparative Examples 1-2, the high resilience sponge materials prepared in Examples 1-3 have better flame retardancy, indicating that two different flame retardant components can achieve better flame retardant effects by combining with each other. In summary, the high resilience sponge materials prepared in the present invention have better market application prospects.
[0109] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0110] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a high resilience sponge material, characterized in that: The preparation method comprises the following steps: S1, using ammonium polyphosphate, alkali lignin and diphenylmethane diisocyanate as raw materials to prepare an intumescent flame retardant component, and using 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and as raw materials to prepare a halogen-free reactive flame retardant component; S2, using polyester polyol block prepolymer and 1,4-butylene diisocyanate as raw materials to prepare self-made polyurethane, then using anhydrous ethanol as a precipitation washing liquid to precipitate and purify the self-made polyurethane, and the obtained precipitate is recorded as solid polyurethane after drying; S3. Weigh 30-35g of solid polyurethane, 18-20g of polyethylene glycol 4000, 26-30g of dioxane and 5-6g of toluene diisocyanate, mix and stir, stir and react at 60°C for 20min, then pour into a mold for foaming, after foaming, place in a freeze dryer at 20°C for freezing at normal pressure for 3h, then place in a vacuum dryer at 25°C for 12h, and the obtained sponge material is a high resilience sponge material.
2. The method for preparing a high resilience sponge material according to claim 1, characterized in that: In S1, the preparation steps of the intumescent flame retardant component are: Step 1, weigh 45g of ammonium polyphosphate and disperse it in a flask filled with 250mL of ethyl acetate, add 10g of diphenylmethane diisocyanate, heat it in a water bath to 50°C, and stir and mix for 1h, then add 5g of alkali lignin, heat it in a water bath to 60°C, and react at this temperature for 5h, the result is recorded as the reaction component; Step 2: Filter the reaction components to remove the filtrate, then wash with ethyl acetate three times, dry and grind through an 80-mesh sieve to obtain an intumescent flame retardant component.
3. The method for preparing a high resilience sponge material according to claim 2, characterized in that: In step one, the stirring speed of the stirring mixture is 300 r / min, and in step two, the drying method is to place the mixture in an oven at 80° C. and dry it for 24 hours.
4. The method for preparing a high resilience sponge material according to claim 1, characterized in that: In S1, the preparation steps of the halogen-free reactive flame retardant component are: Step A, weigh 10g 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 200mL xylene into a flask, heat to 90°C under nitrogen protection, stir to dissolve and then add 20mL formaldehyde dropwise, react at the original temperature for 6h after the addition is completed, and the result is recorded as the reaction system; Step B, cooling the reaction system to room temperature and filtering to obtain a solid product, washing it with anhydrous ethanol for three times, drying it and grinding it through a 200-mesh sieve to obtain a halogen-free reactive flame retardant component.
5. The method for preparing a high resilience sponge material according to claim 4, characterized in that: In step A, the stirring and dissolving method is to stir at a stirring speed of 200 r / min for 10 minutes, the dripping rate in step A is 1 drop / s, and in step B, the drying method is to place in an oven at 65° C. and dry for 5 hours.
6. The method for preparing a high resilience sponge material according to claim 1, characterized in that: In S2, the preparation steps of the polyester polyol block prepolymer are: Step 1, weigh 30g polyethylene glycol, 8g D, L-lactide, 10g trimethylene carbonate and 0.1g stannous octoate into a flask, mix well, evacuate and replace with nitrogen three times, then heat to 130°C and keep warm for 6h, the result is recorded as the block prepolymer component; Step 2: Pour 200 mL of dichloromethane into the block prepolymer component, and then use petroleum ether as a precipitation washing liquid to perform precipitation purification treatment to obtain a polyester polyol block prepolymer wet material, and the obtained polyester polyol block prepolymer is obtained after drying treatment.
7. The method for preparing a high resilience sponge material according to claim 6, characterized in that: In step 1, the method for uniform mixing is to stir at a stirring speed of 150 r / min for 10 minutes. In step 2, the method for drying is to place in a vacuum drying oven at 40° C. and dry for 12 hours.
8. The method for preparing a high resilience sponge material according to claim 1, characterized in that: In S2, the preparation method of the homemade polyurethane is: 1) Weigh 70g of polyester polyol block prepolymer and 30g of 1,4-butanediisocyanate into a reaction kettle, add 1g of N,N′-dimethylformamide, evacuate and replace with nitrogen three times, heat to 80°C and react at constant temperature for 4h, the result is recorded as reaction mixture; 2) Add 0.1 g of stannous octoate and 20 g of 1,4-butanediol to the reaction mixture, evacuate the mixture again and replace it with nitrogen three times, and then react at a constant temperature of 80° C. for 6 h to obtain the self-made polyurethane.
9. The method for preparing a high resilience sponge material according to claim 1, characterized in that: In S2, the drying method is to place the mixture in a vacuum drying oven at 60°C for 10 hours. In S3, the mixing and stirring method is to stir the mixture at a stirring speed of 300 r / min for 10 minutes, and the foaming time is 3-5 minutes.
10. A high resilience sponge material, characterized in that: The sponge material is prepared by the method for preparing a high resilience sponge material according to any one of claims 1 to 9.
Citation Information
Cited By
A high resilience mattress sponge and method of making same
CN120574370B