High-performance polyurethane court material and preparation method thereof
By introducing modified castor oil polyol, end amino polyether and chain extender, combined with isocyanate compounding, the self-catalytic curing of polyurethane field materials is achieved, solving the problem of wear resistance and cumbersome construction, and improving the mechanical properties of the materials and wear resistance simplifies construction technology and reduces maintenance costs.
Patent Information
- Application Number
- CN202411473040.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-10-22
AI Technical Summary
The existing polyurethane stadium materials are not wear-resistant and have short service life, and the two-component materials require catalyst curing, and the construction process of single-component materials is cumbersome, resulting in high maintenance costs.
The modified castor oil polyol, end amino polyether and chain extender are combined to achieve self-catalytic curing of the material through isocyanate in component B, improving mechanical properties and wear resistance, simplifying the construction process, and avoiding the use of catalysts.
High-performance polyurethane stadium materials with high hardness and good wear resistance are obtained, with high construction efficiency, suitable for industrial production, and reduce maintenance costs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polyurethane court materials, and in particular relates to a high-performance polyurethane court material and a preparation method thereof. Background Art
[0002] In recent years, with the vigorous development of national fitness, significant progress has been made in the construction of sports facilities. Polyurethane plastic sports surfaces have been widely used, especially in basketball, badminton, and table tennis courts in communities, parks, and schools. However, in practice, many sports fields currently suffer from wear, aging, and delamination due to their inherent strength and the frequency of activity. This significantly reduces the lifespan of the fields and requires frequent repairs and renovations, increasing maintenance costs.
[0003] At present, polyurethane court materials are divided into two-component and one-component. Two-component materials require additional catalysts to achieve curing when used. If the catalyst is forgotten or added too little during use, the material will not cure, and the problem material will be sticky and have poor strength, which is more troublesome to handle. Although single-component materials do not require catalysts, the thickness of a single coating is required to be less than 2mm. Multiple scrapings are required to reach the designed thickness, and the construction process is cumbersome.
[0004] CN110643015A discloses a highly wear-resistant and high-strength polyurethane court material, its preparation method, and its use method. The material performance is improved by introducing modified carbon nanotubes. However, the modified carbon nanotubes are prepolymerized in the isocyanate B component, and the preparation method does not have a dehydration step. In addition, the use of an organic bismuth catalyst has high catalytic activity, and its storage stability has problems.
[0005] Therefore, it is necessary to develop a two-component polyurethane court material with high strength, good wear resistance and no catalyst. Summary of the Invention
[0006] The purpose of the present invention is to overcome the above-mentioned defects of the prior art, provide a high-performance polyurethane court material, solve the problems of conventional polyurethane courts being not wear-resistant and having a short service life, and the prepared product has excellent mechanical properties and good wear resistance, and the product cures quickly, has strong operability, and does not require the use of a catalyst; secondly, the present invention also provides a preparation method thereof, which has a simple process and is easy to operate.
[0007] The high-performance polyurethane court material of the present invention is composed of component A and component B in a mass ratio of (4.5-5.5):1, wherein component A includes the following raw materials in mass percentage: 20-25% modified castor oil polyol, 5-10% amino-terminated polyether, 0.5-0.7% chain extender, 60-65% filler, 1.5-3% pigment, 0.7-2% anti-settling agent, 2-3.5% water absorbent, 0.2-0.4% dispersant, 0.3-0.5% antioxidant, and 0.3-0.5% ultraviolet absorber; Component B includes the following raw materials in the following mass percentages: 70-80% isocyanate and 20-30% polyether polyol.
[0008] The modified castor oil polyol is an aromatic polyol with a number average molecular weight of 500-1200 and a functionality of 2-3.5, preferably SY798, purchased from Shanghai Shuyu Chemical Co., Ltd.
[0009] The polyether polyol is polyoxypropylene polyol with a number average molecular weight of 1000-3000 and a functionality of 2, preferably INOVOLC220, purchased from Shandong Yinuowei New Materials Co., Ltd.
[0010] The amino-terminated polyether is a primary amino-terminated polypropylene oxide compound, preferably LHD-1200, purchased from Shandong Longhua New Materials Co., Ltd.
[0011] The isocyanate is a mixture of polymeric MDI and diphenylmethane diisocyanate in a mass ratio of (1-2):1, the polymeric MDI is preferably PM-200, and the diphenylmethane diisocyanate is preferably MDI-50, and both PM-200 and MDI-50 are purchased from Yantai Wanhua Chemical Group Co., Ltd.
[0012] The chain extender is one of ethylene glycol and 1,4-butanediol. Ethylene glycol is purchased from Shandong Baihua Chemical Co., Ltd., and 1,4-butanediol is purchased from Wuhan Jixin Yibang Biotechnology Co., Ltd.
[0013] The filler is heavy calcium carbonate with a mesh size of 400, purchased from Jiangxi Guangyuan Chemical Co., Ltd.
[0014] The pigment is iron oxide green, purchased from Shanghai Yipin Pigment Co., Ltd.
[0015] The anti-settling agent is precipitated silica, preferably ZB-3000, purchased from Jinan Zhongbei Fine Chemical Co., Ltd.
[0016] The water absorbent is 3A molecular sieve, purchased from Pingxiang Liya New Materials Co., Ltd.
[0017] The dispersant is a nonionic neutral dispersant, preferably YRFC-03, purchased from Guangzhou Yourun Synthetic Materials Co., Ltd.
[0018] The antioxidant is a hindered phenol antioxidant, preferably Irganox 1135, purchased from BASF.
[0019] The ultraviolet absorber is a benzotriazole ultraviolet absorber, preferably Tinuvin 329, which is purchased from BASF.
[0020] The method for preparing the high-performance polyurethane court material comprises the following steps: (1) Component A: Add modified castor oil polyol, amino-terminated polyether and chain extender into a reactor, stir and heat to 60-70°C, then add filler, pigment, anti-settling agent, ultraviolet absorber and antioxidant, heat to 90-100°C, dehydrate under vacuum of -0.1MPa for 2-3h, then add water absorbent and dispersant, stir for 1-2h to obtain component A.
[0021] (2) Component B: Add isocyanate into the reaction kettle and stir evenly, then add polyether polyol, heat to 80-85℃, keep the temperature to react for 1-2h, and then cool down to obtain component B.
[0022] (3) When in use, mix components A and B according to the mass ratio and spread them on the field. After curing at room temperature, high-performance polyurethane court materials are obtained.
[0023] Compared with the prior art, the present invention has the following beneficial effects: (1) The high-performance polyurethane court material of the present invention, starting from the molecular structure design, introduces modified castor oil polyol, which has an aromatic structure and a long fatty chain structure of plant oils, reduces the polarity of the molecular chain, and gives the material better mechanical properties; on the other hand, the primary amino group is introduced by combining with the end amino polyether, and the small molecule chain extender is coordinated to greatly improve the curing speed of the material, realize the self-catalytic characteristics of the material, and achieve the effect of curing at room temperature without adding a catalyst, thereby improving the construction efficiency, and the prepared product has high hardness and good wear resistance.
[0024] (2) The high-performance polyurethane court material of the present invention, while introducing modified castor oil polyol, terminal amino polyether and chain extender, effectively reduces the viscosity of the liquid through the reasonable compounding of isocyanate in component B, synergistically using low oil absorption filler and non-ionic neutral dispersant, so that the material maintains high activity and high strength while having good operational leveling properties, reducing the difficulty of construction.
[0025] (3) The preparation method of the high-performance polyurethane court material of the present invention has a simple process, can be cured without a catalyst, is easy to operate, and is suitable for industrial production. DETAILED DESCRIPTION
[0026] The present invention will be further described below with reference to the following examples, but they do not limit the implementation of the present invention.
[0027] Unless otherwise specified, the raw materials used in the examples and comparative examples are conventional commercially available raw materials, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.
[0028] Some of the raw materials used in the examples and comparative examples are described as follows: SY798: Shanghai Shuyu Chemical Co., Ltd. LHD-1200: Shandong Longhua New Materials Co., Ltd. PM-200: Yantai Wanhua Chemical Group Co., Ltd. MDI-50: Yantai Wanhua Chemical Group Co., Ltd. INOVOLC220: Shandong Yinuowei New Materials Co., Ltd. Ethylene glycol: Shandong Baihua Chemical Co., Ltd.; 1,4-Butanediol: Wuhan Jixinyibang Biotechnology Co., Ltd.; Heavy calcium carbonate: Jiangxi Guangyuan Chemical Co., Ltd.; Iron oxide green: Shanghai Yipin Pigment Co., Ltd. ZB-3000: Jinan Zhongbei Fine Chemical Co., Ltd. 3A molecular sieve: Pingxiang Liya New Materials Co., Ltd. YRFC-03: Guangzhou Yourun Synthetic Materials Co., Ltd. Irganox 1135: BASF SE; Tinuvin 329: BASF SE; Castor oil: Jinan Haiyuan Chemical Co., Ltd.
[0029] The high-performance polyurethane court material of the present invention is composed of component A and component B in a mass ratio of (4.5-5.5):1, wherein component A comprises the following raw materials in mass percentage: 20-25% modified castor oil polyol, 5-10% amino-terminated polyether, 0.5-0.7% chain extender, 60-65% filler, 1.5-3% pigment, 0.7-2% anti-settling agent, 2-3.5% water absorbent, 0.2-0.4% dispersant, 0.3-0.5% antioxidant, and 0.3-0.5% ultraviolet absorber; Component B includes the following raw materials in the following mass percentages: 70-80% isocyanate and 20-30% polyether polyol.
[0030] The method for preparing the high-performance polyurethane court material comprises the following steps: (1) Component A: Add modified castor oil polyol, amino-terminated polyether and chain extender into a reactor, stir and heat to 60-70°C, then add filler, pigment, anti-settling agent, ultraviolet absorber and antioxidant, heat to 90-100°C, dehydrate under vacuum of -0.1MPa for 2-3h, then add water absorbent and dispersant, stir for 1-2h to obtain component A.
[0031] (2) Component B: Add isocyanate into the reactor and stir evenly, then add polyether polyol, heat to 80-85℃, keep the temperature to react for 1-2h, cool to 60℃ and discharge the material to obtain component B.
[0032] (3) When in use, mix components A and B according to the mass ratio and spread them on the field. After curing at room temperature, high-performance polyurethane court materials are obtained.
[0033] Example 1 The high-performance polyurethane court material is composed of component A and component B in a mass ratio of 5:1, wherein component A includes the following raw materials in mass percentage: 20% SY798, 10% LHD-1200, 0.5% ethylene glycol, 60% heavy calcium carbonate, 3% iron oxide green, 2% ZB-3000, 3.5% 3A molecular sieve, 0.2% YRFC-03, 0.5% Irganox 1135, and 0.3% Tinuvin 329; Component B includes the following raw materials in the following mass percentages: 70% isocyanate (PM-200:MDI-50=1:1), 30% INOVOLC220.
[0034] The method for preparing the high-performance polyurethane court material comprises the following steps: (1) Component A: SY798, LHD-1200 and ethylene glycol were added to a kettle, stirred and heated to 60°C, then heavy calcium carbonate, iron oxide green, ZB-3000, Tinuvin 329 and Irganox 1135 were added, the temperature was raised to 100°C, and dehydrated under vacuum at -0.1 MPa for 2 h. Then 3A molecular sieve and YRFC-03 were added and stirred for 1 h to obtain component A.
[0035] (2) Component B: PM-200 and MDI-50 in a mass ratio of 1:1 are added to the reactor, stirred evenly, and then INOVOLC220 is added. The temperature is raised to 85°C, kept at this temperature for 2 hours, and then cooled to 60°C and discharged to obtain component B.
[0036] (3) When in use, mix components A and B in a mass ratio of 5:1 and spread them on the field. After curing at room temperature, high-performance polyurethane court materials are obtained.
[0037] Example 2 The high-performance polyurethane court material is composed of component A and component B in a mass ratio of 4.5:1, wherein component A includes the following raw materials in mass percentage: 25% SY798, 5% LHD-1200, 0.7% ethylene glycol, 62% heavy calcium carbonate, 2% iron oxide green, 1.2% ZB-3000, 3% 3A molecular sieve, 0.3% YRFC-03, 0.4% Irganox 1135, and 0.4% Tinuvin 329; Component B includes the following raw materials in the following mass percentages: 80% isocyanate (PM-200:MDI-50=2:1), 20% INOVOLC220.
[0038] The preparation method of the high-performance polyurethane court material comprises the following steps: (1) Component A: SY798, LHD-1200 and ethylene glycol were added to a kettle, stirred and heated to 70°C, then heavy calcium carbonate, iron oxide green, ZB-3000, Tinuvin 329 and Irganox 1135 were added, the temperature was raised to 90°C, and dehydrated under vacuum at -0.1 MPa for 3 h. Then 3A molecular sieve and YRFC-03 were added and stirred for 1.5 h to obtain component A.
[0039] (2) Component B: PM-200 and MDI-50 in a mass ratio of 2:1 were added into a reactor, stirred evenly, and then INOVOLC220 was added. The temperature was raised to 80°C, kept at this temperature for 1 hour, and then cooled to 60°C and discharged to obtain component B.
[0040] (3) When in use, mix components A and B in a mass ratio of 4.5:1 and spread them on the field. After curing at room temperature, high-performance polyurethane court materials are obtained.
[0041] Example 3 The high-performance polyurethane court material is composed of component A and component B in a mass ratio of 5.5:1, wherein component A includes the following raw materials in mass percentage: 22% SY798, 7% LHD-1200, 0.6% 1,4-butanediol, 65% heavy calcium carbonate, 1.5% iron oxide green, 0.7% ZB-3000, 2% 3A molecular sieve, 0.4% YRFC-03, 0.3% Irganox 1135, and 0.5% Tinuvin 329; Component B includes the following raw materials in the following mass percentages: 75% isocyanate (PM-200:MDI-50=1.5:1), 25% INOVOLC220.
[0042] The method for preparing the high-performance polyurethane court material comprises the following steps: (1) Component A: SY798, LHD-1200 and 1,4-butanediol were added to a kettle, stirred and heated to 65°C, then heavy calcium carbonate, iron oxide green, ZB-3000, Tinuvin 329 and Irganox 1135 were added, the temperature was raised to 95°C, and dehydrated under vacuum at -0.1 MPa for 2.5 h. Then 3A molecular sieve and YRFC-03 were added and stirred for 1 h to obtain component A.
[0043] (2) Component B: PM-200 and MDI-50 in a mass ratio of 1.5:1 were added to the reactor, stirred evenly, and then INOVOLC220 was added. The temperature was raised to 83°C, kept warm for 1.5 hours, and then cooled to 60°C and discharged to obtain component B.
[0044] (3) When in use, mix components A and B in a mass ratio of 5.5:1 and spread them on the field. After curing at room temperature, high-performance polyurethane court materials are obtained.
[0045] Comparative Example 1 This comparative example is the same as Example 1, except that SY798 in component A is replaced by castor oil. In Comparative Example 1, component A includes the following raw materials in percentage by mass: 24% castor oil, 10% LHD-1200, 0.5% ethylene glycol, 56% heavy calcium carbonate, 3% iron oxide green, 2% ZB-3000, 3.5% 3A molecular sieve, 0.2% YRFC-03, 0.5% Irganox 1135, and 0.3% Tinuvin329; the raw materials of component B and their percentage by mass, and the preparation method of the high-performance polyurethane court material are the same as those in Example 1.
[0046] Comparative Example 2 This comparative example is the same as Example 1, except that the amino-terminated polyether LHD-1200 in component A is replaced by INOVOL C220 of the same mass percentage. In Comparative Example 2, component A includes the following raw materials in mass percentage: 20% SY798, 10% INOVOLC220, 0.5% ethylene glycol, 60% heavy calcium carbonate, 3% iron oxide green, 2% ZB-3000, 3.5% 3A molecular sieve, 0.2% YRFC-03, 0.5% Irganox 1135, and 0.3% Tinuvin 329; the raw materials of component B and their mass percentages, and the preparation method of the high-performance polyurethane court material are the same as those in Example 1.
[0047] Comparative Example 3 This comparative example is the same as Example 1, except that SY798 in component A is replaced by castor oil and the amino-terminated polyether LHD-1200 is removed. In Comparative Example 3, component A includes the following raw materials in percentage by mass: 24% castor oil, 10% INOVOLC220, 0.5% ethylene glycol, 56% heavy calcium carbonate, 3% iron oxide green, 2% ZB-3000, 3.5% 3A molecular sieve, 0.2% YRFC-03, 0.5% Irganox 1135, and 0.3% Tinuvin 329; the raw materials of component B and their percentage by mass, and the preparation method of the high-performance polyurethane court material are the same as those in Example 1.
[0048] Comparative Example 4 This comparative example is the same as Example 1, except that the isocyanate mixture (PM-200:MDI-50=1:1) in component B is replaced with PM-200 of the same mass percentage. The remaining raw material proportions and preparation methods are the same as those in Example 1.
[0049] Comparative Example 5 The difference from Example 1 is that the process of adding the water-absorbing agent 3A molecular sieve in the preparation method is different.
[0050] The raw material compositions and mass percentages of component A and component B are the same as those in Example 1.
[0051] The method for preparing the high-performance polyurethane court material comprises the following steps: (1) Component A: SY798, LHD-1200 and ethylene glycol were added to a reactor, stirred and heated to 60°C, and then heavy calcium carbonate, 3A molecular sieve, iron oxide green, ZB-3000, Tinuvin 329 and Irganox 1135 were added. The temperature was raised to 100°C, and the mixture was dehydrated under a vacuum of -0.1 MPa for 2 h. YRFC-03 was then added and stirred for 1 h to obtain component A.
[0052] (2) Component B: PM-200 and MDI-50 in a mass ratio of 1:1 are added to the reactor, stirred evenly, and then INOVOLC220 is added. The temperature is raised to 85°C, kept at this temperature for 2 hours, and then cooled to 60°C and discharged to obtain component B.
[0053] (3) When in use, mix components A and B in a mass ratio of 5:1 and spread them on the field. After curing at room temperature, high-performance polyurethane court materials are obtained.
[0054] The polyurethane court materials prepared in Examples 1-3 and Comparative Examples 1-5 were subjected to performance testing. The operating time was tested according to GB / T7123.1-2015, the tensile strength and elongation at break were tested according to GB / T528-2009, the hardness was tested according to GB / T2411-2008, and the wear resistance was tested according to GB / T1768-2006 (test conditions: rubber grinding wheel model CS-10F, load 500g, rotation speed 1000r). The test results are shown in Table 1.
[0055] Table 1 Test results
[0056] As can be seen from Table 1, the high-performance polyurethane court materials prepared in Examples 1-3 exhibit significant performance advantages over the comparative examples. The mechanical properties and wear resistance of the polyurethane court material prepared in Comparative Example 1 were reduced due to the lack of aromatic structure in the castor oil molecular chain, resulting in reduced product activity and poorer mechanical properties and wear resistance. Substituting the amino-terminated polyether in Comparative Example 2 also resulted in a corresponding decrease in activity. The polyurethane court material prepared in Comparative Example 3 exhibited a long operating time and the worst performance. This is because the use of castor oil and polyether polyols without a catalyst results in low product activity, inability to achieve autocatalysis, and slow curing, resulting in poor crosslinking strength and failure to meet field use requirements. In Comparative Example 4, replacing the isocyanate mixture with PM-200 alone resulted in increased product activity, shortened operating time, and impracticality for on-site paving. In Comparative Example 5, adjusting the process to change the order of addition of the water-absorbing agent 3A molecular sieve resulted in significantly reduced mechanical properties. This is because the water-absorbing agent was added before dehydration, absorbing a large amount of water, reducing its own water absorption capacity, causing foaming in the product and degrading its physical properties. Comparison of Comparative Examples 1-5 shows that, by introducing modified castor oil polyol, amino-terminated polyether and chain extender, the rational compounding of isocyanate in component B, synergistically using low oil absorption filler and non-ionic neutral dispersant and water absorbent, the operational leveling is effectively improved, and self-catalysis can be achieved without a catalyst. The prepared product has excellent mechanical properties, good wear resistance, strong operability and fast curing time.
Claims
1. A high-performance polyurethane court material, characterized in that: The method comprises component A and component B in a mass ratio of (4.5-5.5):1, wherein component A comprises the following raw materials in mass percentage: 20-25% modified castor oil polyol, 5-10% amino-terminated polyether, 0.5-0.7% chain extender, 60-65% filler, 1.5-3% pigment, 0.7-2% anti-settling agent, 2-3.5% water absorbent, 0.2-0.4% dispersant, 0.3-0.5% antioxidant, and 0.3-0.5% ultraviolet absorber; Component B includes the following raw materials in percentage by mass: 70-80% isocyanate, 20-30% polyether polyol; The modified castor oil polyol is an aromatic polyol with a number average molecular weight of 500-1200 and a functionality of 2-3.5; The amino-terminated polyether is a primary amino-terminated polypropylene oxide compound; The isocyanate is a mixture of polymeric MDI and diphenylmethane diisocyanate.
2. The high-performance polyurethane court material according to claim 1, characterized in that: The polyether polyol is polyoxypropylene polyol with a number average molecular weight of 1000-3000 and a functionality of 2.
3. The high performance polyurethane court material according to claim 1, characterized in that: The chain extender is one of ethylene glycol and 1,4-butanediol.
4. The high performance polyurethane court material according to claim 1, characterized in that: The filler is heavy calcium carbonate and the pigment is iron oxide green.
5. The high performance polyurethane court material according to claim 1, characterized in that: The anti-settling agent is precipitated silica, and the water absorbent is 3A molecular sieve.
6. The high performance polyurethane court material according to claim 1, characterized in that: The dispersant is a nonionic neutral dispersant.
7. The high performance polyurethane court material according to claim 1, characterized in that: The antioxidant is a hindered phenol antioxidant.
8. The high performance polyurethane court material according to claim 1, characterized in that: The ultraviolet absorber is a benzotriazole ultraviolet absorber.
9. The high performance polyurethane court material according to claim 1, characterized in that: The isocyanate is a mixture of polymeric MDI and diphenylmethane diisocyanate, and the mass ratio of the two is (1-2):
1.
10. A method for preparing the high-performance polyurethane court material according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Component A: Add modified castor oil polyol, amino-terminated polyether and chain extender into a reaction kettle, stir and heat to 60-70°C, then add filler, pigment, anti-settling agent, ultraviolet absorber and antioxidant, heat to 90-100°C, dehydrate for 2-3 hours under vacuum degree of -0.1MPa, then add water absorbent and dispersant, stir for 1-2 hours, and obtain component A; (2) Component B: Add isocyanate into the reaction kettle, stir evenly, then add polyether polyol, raise the temperature to 80-85°C, keep the temperature to react for 1-2 hours, and then cool down to obtain component B; (3) When in use, mix components A and B according to the mass ratio and spread them on the field. After curing at room temperature, high-performance polyurethane court material is obtained.
Citation Information
Patent Citations
High-wear-resistance and high-strength polyurethane court material, and preparation method and using method thereof
CN110643015A
Solvent-free polyurethane floor paint and preparation method thereof
CN108300276A
Polyurethane grouting material for simultaneously lifting and rectifying high-speed railway ballastless track
CN108359122A
Alkali-resistant and salt-resistant polyurethane plastic basketball scene surface layer material and preparation method thereof
CN116199854A
Two-component coating composition
EP3988597A1
Cited By
Polyurethane plastic track surface layer material and preparation method for improving weather resistance of polyurethane plastic track surface layer material