Bio-based benzoxazine monomer modified epoxy resin and preparation method thereof

By using a combination of bio-based benzoxazine phosphate monomer, Priamine 1074 and DGEBA, the problem of insufficient mechanical strength and thermal stability of epoxy resin was solved, and a bio-based with high tensile strength and flame retardant properties was prepared. Benzoxazine monomer modified epoxy resin, suitable for a variety of high-performance materials.

CN118978669AActive Publication Date: 2024-11-19INST OF CHEM IND OF FOREST PROD CHINESE ACAD OF FORESTRY

Patent Information

Application Number
CN202411302461.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-19
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The existing epoxy resins have shortcomings in mechanical strength and thermal stability, and the curing agent Priamine 1074 of traditional benzoxazine resins has problems such as low crosslinking density, flammability, difficulty in degradation and low mechanical strength.

Method used

Bio-based benzoxazine phosphate monomer TBP, bio-based diamine Priamine 1074 and bisphenol A diglycidyl ester DGEBA were used as raw materials, and bio-based benzoxazine monomer modification was prepared through specific reaction steps and conditions. epoxy resin increases molecular chain rigidity and nitrogen and phosphorus content to form a resin with high tensile strength, thermal stability and flame retardant properties.

Benefits of technology

The prepared bio-based benzoxazine monomer modified epoxy resin has high tensile strength, excellent thermal stability and flame retardant properties, and is degradable under alkaline conditions. It is suitable for flame retardant materials and carbon fibers. Reinforced composites and low dielectric materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978669A_ABST
    Figure CN118978669A_ABST
Patent Text Reader

Abstract

The invention discloses bio-based benzoxazine monomer modified epoxy resin and a preparation method thereof. The preparation method comprises the following steps: reacting guaiacol, ethanolamine and paraformaldehyde to obtain a bio-based benzoxazine monomer; the preparation method comprises the following steps: reacting a bio-based benzoxazine monomer with phosphorus oxychloride in a solvent to obtain a benzoxazine phosphate monomer; the preparation method comprises the following steps: by taking benzoxazine phosphate as a modified curing agent and bio-based diamine Priamine 1074 as a toughening curing agent, uniformly mixing the benzoxazine phosphate and the bio-based diamine Priamine 1074 with bisphenol A epoxy resin DGEBA, pouring the mixture into a mold, and then heating and curing to obtain the bio-based benzoxazine monomer modified epoxy resin. The bio-based benzoxazine monomer modified epoxy resin obtained by the invention has relatively strong mechanical properties and thermal stability, and also shows excellent adhesion performance, flame retardant property, low dielectric property and degradability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a bio-based benzoxazine monomer modified epoxy resin and a preparation method thereof, belonging to the technical field of natural resource modification. Background Art

[0002] As people pay more and more attention to global resources and environmental issues, coupled with the rapid consumption of petroleum energy, energy crisis and environmental problems have become an issue that cannot be avoided and must be addressed head-on. Finding natural renewable resources to replace traditional petroleum raw materials to synthesize polymer materials has become a research hotspot. Guaiacol and Priamine 1074 are derived from lignin degradation phenols and plant oil extracts, respectively, and are both renewable forestry biomass resources. Although Priamine 1074 can be used as a curing agent for epoxy resin, its low cross-linking density, poor thermal stability, flammability, difficulty in degradation and low mechanical strength limit its application.

[0003] Benzoxazine resin is a new type of thermosetting resin developed on the basis of traditional phenolic resin. It has the advantages of flexible molecular design, excellent thermal stability and low dielectric properties. It has application potential in aerospace, hydrophobic flame retardant, anticorrosive and antibacterial, electronic communications and other fields. Unlike traditional thermosetting resins, benzoxazine resins can be made from natural renewable resources in addition to fossil raw materials. At present, benzoxazine resins have synthesized monomers from renewable resources and have made breakthroughs in raw material sources and performance improvements. Various active groups can be introduced by using its flexible molecular design. At the same time, benzoxazine monomers will form a large number of phenolic hydroxyl and tertiary amine groups during the ring opening process. Phenolic hydroxyl groups can participate in the ring opening reaction of epoxy groups to form a cross-linked network structure, and tertiary amine groups can promote the reaction; in addition, the benzoxazine skeleton can further improve the rigidity and thermal stability of the molecular chain. Therefore, benzoxazine monomers are an excellent epoxy resin modified curing agent. Summary of the invention

[0004] In order to solve the defects of epoxy resin in the prior art such as low mechanical strength and poor thermal stability, the present invention provides a bio-based benzoxazine monomer modified epoxy resin and a preparation method thereof. The prepared bio-based benzoxazine monomer modified epoxy resin increases the molecular chain rigidity and nitrogen and phosphorus content of the resin, so that the resin has higher tensile strength, excellent thermal stability and excellent non-flammability. The introduction of phosphate bonds gives the resin better flame retardancy and recyclability. At the same time, the resin also has good hydrophobicity, adhesion and low dielectric properties.

[0005] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows:

[0006] A bio-based benzoxazine monomer modified epoxy resin, characterized in that: its raw material components include: bio-based benzoxazine phosphate monomer TBP, bio-based diamine Priamine 1074 and bisphenol A diglycidyl ester DGEBA;

[0007] The structural formulas are:

[0008]

[0009] The present invention also provides a method for preparing a bio-based benzoxazine monomer modified epoxy resin, comprising the following steps:

[0010] (1) reacting guaiacol, ethanolamine and paraformaldehyde to obtain a bio-based benzoxazine monomer;

[0011] (2) adding a bio-based benzoxazine monomer and phosphorus oxychloride into a solvent for reaction to obtain a bio-based benzoxazine phosphate monomer;

[0012] (3) mixing the bio-based benzoxazine phosphate monomer, the bio-based diamine Priamine 1074 and bisphenol A diglycidyl ester evenly and pouring the mixture into a mold, and then heating and curing the mixture to obtain a bio-based benzoxazine monomer modified epoxy resin;

[0013] The reaction process is:

[0014]

[0015] Preferably, the reaction temperature in step (1) is 60° C. to 90° C., and the reaction time is 12 to 18 hours.

[0016] Preferably, the reaction temperature in step (2) is 0°C to 10°C, and the reaction time is 24 to 36 hours.

[0017] Preferably, the molar ratio of the sum of the molar amount of the oxazine ring of the bio-based benzoxazine phosphate monomer and the molar amount of the active hydrogen of the bio-based diamine Priamine 1074 to the epoxy group of bisphenol A diglycidyl ester is 1:1.

[0018] Preferably, the mass ratio of the phosphorus content of the bio-based benzoxazine phosphate monomer to the sum of the bio-based benzoxazine phosphate monomer, the bio-based diamine Priamine 1074 and bisphenol A diglycidyl ester is 0.95:100 to 2.46:100.

[0019] Preferably, the curing reaction in step (3) is a self-catalytic reaction system.

[0020] Preferably, the guaiacol, paraformaldehyde and bio-based diamine Priamine 1074 are derived from lignin, biomethanol and vegetable oil, respectively.

[0021] Preferably, the temperature rising and curing procedure is:

[0022] After pre-curing at 60-100°C for 4-8 hours, cure at 100-150°C for 4-6 hours, and finally cure at 150-200°C for 2-4 hours, then cool down.

[0023] Preferably, the cooling process is to cool down to room temperature at a cooling rate of 5 to 8°C / min.

[0024] The technologies not mentioned in the present invention are all referred to the prior art.

[0025] (1) The bio-based benzoxazine monomer modified epoxy resin of the present invention has strong mechanical properties and good thermal stability, as well as excellent adhesion, hydrophobicity, flame retardancy and degradation performance. The tensile strength at room temperature can reach 53MPa and the tensile modulus can reach 875MPa. The temperature of thermal weight loss of 5% is higher than 316°C, and the carbon residue rate at 800°C is 37.4%, which is far higher than that of Priamine 1074 cured bisphenol A epoxy resin DGEBA without adding benzoxazine monomer. At the same time, it can reach V-0 level in UL-94 flame retardancy test, LOI is 32.5%, water contact angle is as high as 117°, and it can be completely degraded under alkaline conditions at 120°C.

[0026] (2) The preparation method of the bio-based benzoxazine monomer modified epoxy resin of the present invention comprises adding trifunctional benzoxazine phosphate (TBP) and Priamine 1074 formed by the reaction of benzoxazine monomer (GE) with phosphorus oxychloride to bisphenol A diglycidyl ester (DGEBA) for curing. The bio-based product is used as a modified curing agent in the synthesis of thermosetting resins, which reduces the use of petroleum-based compounds and conforms to the concept of green development. The obtained bio-based benzoxazine monomer modified epoxy resin can be used in the fields of flame retardant materials, carbon fiber reinforced composite materials, adhesives and low dielectric materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 are the FT-IR patterns of GU, EA, GE, and TBP;

[0028] Figure 2 are the FT-IR patterns of TBP, DGEBA, and EP-TBP-2.46%;

[0029] Figure 3 It is the DMA graph of epoxy resin modified with different proportions of bio-based benzoxazine monomer;

[0030] Figure 4 It is the tensile diagram of epoxy resin modified with different proportions of bio-based benzoxazine monomer;

[0031] Figure 5 is the TGA graph of epoxy resin modified with different proportions of bio-based benzoxazine monomer;

[0032] Figure 6 is a shear diagram of epoxy resin modified with different proportions of bio-based benzoxazine monomer;

[0033] Figure 7 It is the UL-94 vertical burning diagram of epoxy resin modified with different proportions of bio-based benzoxazine monomer;

[0034] Figure 8 The water contact angle diagram of epoxy resin modified with bio-based benzoxazine monomers in different proportions before and after immersion in water for 10 days;

[0035] Fig. 9 It is the dielectric property diagram of EP-TBP-2.46%;

[0036] Fig.10 FT-IR graphs of EP-TBP-2.46% before and after degradation in ethanolamine. DETAILED DESCRIPTION

[0037] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0038] FT-IR (Fourier transform infrared spectroscopy) was performed using a Nicolet IS50 infrared spectrometer with a scanning wavelength from 4000 cm -1 -400cm -1 .

[0039] The tensile test is carried out according to GB13022-91 standard.

[0040] DMA (dynamic thermomechanical analysis) uses TADMAQ800 dynamic thermomechanical analyzer in tensile mode for dynamic thermomechanical analysis. The sample is cut into a rectangular strip with a cross section of 5mm×1mm, and the distance between the clamps is 18mm. The analysis is carried out at a heating rate of 3℃ / min at -50~150℃ and 1Hz frequency, and the changes in storage modulus, loss modulus and tanδ are recorded.

[0041] TGA (thermogravimetric analysis) nitrogen was used as the protective gas, and the heating rate was 10°C / min, from 25°C to 800°C.

[0042] The contact angle test was measured using a Drop Meter A-200 contact angle meter.

[0043] The shear test method is as follows: First, a 100 mm × 25 mm × 1 mm stainless steel substrate was cleaned with deionized water and isopropyl alcohol. Then, a mixture of uncured TBP, Priamine 1074 and DGEBA was applied between two polished stainless steel substrates, bonded, with an overlap area of ​​12.5 mm × 25 mm and a thickness of 0.2 mm, and finally cured.

[0044] The UL-94 vertical burning test was conducted according to ASTM D3801 on a CZF-5 burning test machine (Beijing Zhuorui Technology Co., Ltd., China), with a specimen size of 130 × 13 × 3 mm 3 .

[0045] The dielectric properties were tested using an Agilent 4294A precision impedance analyzer with a frequency range of 1 MHz to 10 MHz.

[0046] Example 1

[0047] A bio-based benzoxazine monomer, the synthesis route of which is:

[0048]

[0049] A method for preparing a bio-based benzoxazine monomer comprises the following steps:

[0050] The starting materials 10g of guaiacol (GU), 4.92g of ethanolamine (EA) and 4.84g of paraformaldehyde were added to a round-bottom flask, and chloroform was used as a solvent to react at 70°C for 20h. After the reaction, it was washed three times with NaOH and three times with deionized water, and then recrystallized in ethanol to obtain a white powder: bio-based benzoxazine monomer (GE).

[0051] A bio-based trifunctional benzoxazine phosphate monomer, the synthesis route of which is:

[0052]

[0053] A method for preparing a bio-based trifunctional benzoxazine phosphate monomer comprises the following steps:

[0054] 10g of bio-based benzoxazine monomer (GE) and 4.84g of triethylamine were dissolved in dichloromethane, and 2.44g of phosphorus oxychloride was added dropwise in an ice-water bath at 0-5°C. After stirring for 30min, the mixture was reacted at room temperature for 30h. After the reaction, the mixture was washed three times with saturated sodium chloride, washed three times with deionized water, and recrystallized with ethanol to obtain a white powder: bio-based trifunctional benzoxazine phosphate monomer (TBP).

[0055] The FT-IR images of GU, EA, GE and TBP are shown in Figure 1 As shown, GU is at 3515cm-1 The characteristic peaks of phenolic hydroxyl group and EA at 3289cm -1 and 3166cm -1 The amino doublet at 3377 cm -1 The alcohol hydroxyl peak at 1210 cm -1 and 1073cm -1 The COC stretching vibration peak of the oxazine ring appeared at 922 cm -1 The absorption peak at 3377 cm is the characteristic peak of the oxazine ring, which proves the successful synthesis of GE. -1 The characteristic peak of alcohol hydroxyl group at 1259 cm-1 completely disappeared, and the absorption peak of P=O group appeared at 1259 cm-1. -1 The absorption peak of PO bond appears at 1018 cm -1 And the characteristic absorption peak of the oxazine ring was retained, proving that TBP was successfully synthesized by the reaction of GE and phosphorus oxychloride.

[0056] The preparation process of bio-based benzoxazine monomer modified epoxy resin is as follows:

[0057] 3.8g of bio-based trifunctional benzoxazine phosphate (TBP) and 10g of bisphenol A epoxy resin (DGEBA) were fully mixed in DMSO at 80°C. After mixing evenly, the excess DMSO was evaporated, and then 4.6g of Priamine 1074 was added and stirred evenly, and then quickly poured into a PTFE mold. Pre-cured at 80°C for 6h, then cured at 120°C for 3h, cured at 150°C for 3h, and finally cured at 180°C for 1 hour. Then cooled to room temperature at a rate of 6°C / min to obtain a bio-based benzoxazine monomer modified epoxy resin (EP-TBP-0.95%).

[0058] Example 2

[0059] The preparation method of bio-based trifunctional benzoxazine phosphate monomer (TBP) is based on Example 1.

[0060] The preparation process of bio-based benzoxazine monomer modified epoxy resin is as follows:

[0061] 7.6g of bio-based trifunctional benzoxazine phosphate (TBP) and 10g of bisphenol A epoxy resin (DGEBA) were fully mixed in DMSO at 80°C. After mixing evenly, the excess DMSO was evaporated, and then 2.3g of Priamine 1074 was added and stirred evenly, and then quickly poured into a PTFE mold. Pre-cured at 80°C for 6h, then cured at 120°C for 3h, cured at 150°C for 3h, and finally cured at 180°C for 1 hour. Then cooled to room temperature at a rate of 6°C / min to obtain a bio-based benzoxazine monomer modified epoxy resin (EP-TBP-1.76%).

[0062] Example 3

[0063] The preparation method of bio-based trifunctional benzoxazine phosphate monomer (TBP) is based on Example 1.

[0064] The preparation process of bio-based benzoxazine monomer modified epoxy resin is as follows:

[0065] 11.4 g of bio-based trifunctional benzoxazine phosphate (TBP) and 10 g of bisphenol A epoxy resin (DGEBA) were fully mixed in DMSO at 80°C, and the excess DMSO was evaporated after mixing evenly, and then quickly poured into a PTFE mold. Pre-cured at 80°C for 6 hours, then cured at 120°C for 3 hours, cured at 150°C for 3 hours, and finally cured at 180°C for 1 hour. Then cooled to room temperature at a rate of 6°C / min to obtain a bio-based benzoxazine monomer modified epoxy resin (EP-TBP-2.46%).

[0066] The FT-IR images of TBP, DGEBA and EP-TBP-2.46% are shown in Figure 2 As shown, EP-TBP-2.46% at 3375 cm -1 The hydroxyl absorption peak at 922 cm -1 The characteristic absorption peak of the oxazine ring at 916 cm -1 The epoxy characteristic absorption peaks at the junction completely disappeared. The changes in these characteristic peaks confirmed the successful preparation of bio-based benzoxazine monomer modified epoxy resin (EP-TBP-2.46%).

[0067] Comparative Example

[0068] The preparation process of bio-based diamine Priamine 1074 cured epoxy resin is as follows:

[0069] 6.9 g of Priamine 1074 and 10 g of bisphenol A epoxy resin (DGEBA) were stirred thoroughly to make them uniform, and then quickly poured into a PTFE mold. Pre-cured at 80°C for 6 h, then cured at 120°C for 3 h, and then cured at 150°C for 3 h. Then cooled to room temperature at a rate of 6°C / min to obtain bio-based diamine Priamine 1074 cured epoxy resin (EP-TBP-0%).

[0070] DMA chart of bio-based benzoxazine monomer modified epoxy resin Figure 3 As shown in a, it can be seen from the figure that the bio-based benzoxazine monomer modified epoxy resin shows a transition from glassy state to rubbery state. At 25°C, the storage modulus (E') of EP-TBP-2.46% is 4720MPa, while that of EP-TBP-0% is only 1188MPa, which is 1 / 4 of that of EP-TBP-2.46%. Figure 3 b It can be seen that with the increase of TBP content, the T g The T of EP-TBP-2.46% g The T of EP-TBP-0% is 113.7℃, which is much higher than that of EP-TBP-0%. g (56℃).

[0071] The tensile curves of epoxy resin modified with different proportions of bio-based benzoxazine monomer are shown in Figure 2. Figure 4 As shown in the figure, it can be seen that the tensile modulus of the bio-based benzoxazine monomer modified epoxy resin increases with the increase of TBP, while the elongation at break is the opposite. Among them, EP-TBP-1.76% has the largest tensile strength of 53MPa. The tensile strength and modulus of EP-TBP-2.46% with the highest TBP content are 49MPa and 875MPa, respectively, and its tensile strength and tensile modulus are 4 times and 13 times that of EP-TBP-0% without TBP.

[0072] The TGA graphs of epoxy resin modified with different proportions of bio-based benzoxazine monomer are shown in Figure 2. Figure 5 As shown in the figure, it can be seen that the thermal stability of the bio-based benzoxazine monomer modified epoxy resin increases with the increase of TBP addition. Compared with EP-TBP-0% without TBP, the T 5% It increased from 192°C to 296°C, an increase of 104°C. Moreover, its carbon residue rate at 800°C (37.4%) reached 47 times that of EP-TBP-0% (0.8%). This is due to the introduction of TBP, which improves the thermal stability of the polymer.

[0073] Shear diagrams of epoxy resin modified with different proportions of bio-based benzoxazine monomers are shown in Figure 2. Figure 6As shown in the figure, it can be seen that the shear strength of the epoxy resin modified with the bio-based benzoxazine monomer first increases and then decreases with the increase of TBP addition, reaching a maximum value of 9.8MPa at EP-TBP-1.76%, showing excellent adhesion to metals. This change pattern is consistent with the tensile strength.

[0074] UL-94 vertical burning test of epoxy resin modified with different proportions of bio-based benzoxazine monomers Figure 7 As shown in the figure, it can be seen that the flame retardancy of the bio-based benzoxazine monomer modified epoxy resin increases with the increase of TBP addition. Among them, the flame retardant grade of EP-TBP-0% without TBP and EP-TBP-0.95% with a phosphorus content of 0.95% is NR, and there is no flame retardant effect. When the phosphorus content reaches 1.76%, that is, the flame retardant grade of EP-TBP-1.76% can reach V-0, and there is no droplet falling. It shows that the introduction of TBP can greatly improve the flame retardant properties of the polymer.

[0075] The water contact angle of the bio-based benzoxazine monomer modified epoxy resin before and after immersion in water for one week is shown in the figure below. Figure 8 As shown in the figure, it can be seen that the water contact angle of the bio-based benzoxazine monomer modified epoxy resin increases with the increase of TBP addition. The water contact angle of EP-TBP-2.46% before being soaked in water is the largest, which is 117°. After soaking in water for one week, the water contact angle of EP-TBP-2.46% decreases slightly to 111°. However, the water contact angle of EP-TBP-0% decreases significantly, from the original 92° to 77°, a decrease of 27.2%. The above results show that the polymer is more hydrophobic after adding TBP.

[0076] In addition, the dielectric constant of EP-TBP-2.46% at 10 MHz is 3.5 and the dielectric loss is 0.0008 ( Fig. 9 ), has good dielectric properties and is suitable for high-frequency electronic packaging materials.

[0077] The degradation process of the bio-based benzoxazine monomer modified epoxy resin is as follows: 5 g of the sample (EP-TBP-2.46%) is added to a single-necked flask, followed by a mixed solution of 20 mL of 1N NaOH and 40 mL of ethanolamine, the temperature is raised to 120°C, and the mixture is stirred sufficiently. After the sample is fully degraded, the solvent is evaporated to obtain the degradation product of EP-TBP-2.46%.

[0078] FT-IR images of EP-TBP-2.46% before and after degradation are shown in Figure 2. Fig.10 As shown in the figure, it can be seen that the degradation product of EP-TBP-2.46% is at 3285 cm -1 The absorption peaks at 1259 cm- -1The P=O bond absorption peak at 1182 cm -1 , indicating that the phosphate bond was amidated by ethanolamine, thus achieving rapid degradation.

[0079] The bio-based benzoxazine monomer modified epoxy resin (EP-TBP polymer) prepared by the present invention has strong mechanical properties and thermal stability, and also has excellent adhesion, flame retardancy, hydrophobicity and degradability. The tensile strength at room temperature can reach 53MPa, and the tensile modulus reaches 875MPa. The temperature of thermal weight loss of 5% is higher than 296°C, the carbon residue rate at 800°C reaches 37.4%, and the UL-94 vertical combustion reaches V-0, which are far higher than Priamine1074 cured epoxy resin DGEBA (EP-TBP-0%) without adding benzoxazine monomer (TBP). In addition, the shear strength of EP-TBP polymer to metal can reach 9.8MPa, the water contact angle is as high as 117°, the dielectric loss is as low as 0.0008, and it can be rapidly amidated under alkaline conditions to achieve degradation.

[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A bio-based benzoxazine monomer modified epoxy resin, characterized in that: Its raw material components include: bio-based benzoxazine phosphate monomer TBP, bio-based diamine Priamine 1074 and bisphenol A diglycidyl ester DGEBA; The structural formulas are:

2. The method for preparing a bio-based benzoxazine monomer modified epoxy resin according to claim 1, characterized in that: The following steps are involved: (1) reacting guaiacol, ethanolamine and paraformaldehyde to obtain a bio-based benzoxazine monomer; (2) adding a bio-based benzoxazine monomer and phosphorus oxychloride into a solvent for reaction to obtain a bio-based benzoxazine phosphate monomer; (3) The bio-based benzoxazine phosphate monomer, the bio-based diamine Priamine 1074 and bisphenol A diglycidyl ester are uniformly mixed and poured into a mold, and then heated and cured to obtain a bio-based benzoxazine monomer modified epoxy resin.

3. The method for preparing a bio-based benzoxazine monomer modified epoxy resin according to claim 2, characterized in that: The reaction temperature in step (1) is 60° C. to 90° C., and the reaction time is 12 to 18 hours.

4. The method for preparing a bio-based benzoxazine monomer modified epoxy resin according to claim 2, characterized in that: The reaction temperature in step (2) is 0°C to 10°C, and the reaction time is 24 to 36 hours.

5. The method for preparing a bio-based benzoxazine monomer modified epoxy resin according to claim 2, characterized in that: The molar ratio of the sum of the molar amount of the oxazine ring of the bio-based benzoxazine phosphate monomer and the molar amount of the active hydrogen of the bio-based diamine Priamine 1074 to the epoxy group of bisphenol A diglycidyl ester is 1:

1.

6. The method for preparing a bio-based benzoxazine monomer modified epoxy resin according to claim 2 or 5, characterized in that: The mass ratio of the phosphorus content of the bio-based benzoxazine phosphate monomer to the total of the bio-based benzoxazine phosphate monomer, the bio-based diamine Priamine 1074 and bisphenol A diglycidyl ester is 0.95:100 to 2.46:

100.

7. The method for preparing a bio-based benzoxazine monomer modified epoxy resin according to claim 2, characterized in that: The curing reaction in step (3) is a self-catalytic reaction system.

8. The method for preparing a bio-based benzoxazine monomer modified epoxy resin according to claim 2, characterized in that: The guaiacol, polyformaldehyde and diamine Priamine 1074 are derived from lignin, biomethanol and vegetable oil respectively.

9. The method for preparing a bio-based benzoxazine monomer modified epoxy resin according to claim 2, characterized in that: The temperature rise curing procedure is: After pre-curing at 60-100°C for 4-8 hours, cure at 100-150°C for 4-6 hours, and finally cure at 150-200°C for 2-4 hours, then cool down.

10. The method for preparing a bio-based benzoxazine monomer modified epoxy resin according to claim 9, characterized in that: The cooling process is to cool the temperature to room temperature at a cooling rate of 5 to 8°C / min.

Citation Information

Patent Citations

  • Halogen-free fire-resistant epoxy resin composition, film and copper clad laminate

    CN101302327A

  • DOPO-containing bisphenol A-monobenzoxazine / epoxy resin copolymer and preparation method thereof

    CN104193967A

  • Phosphorus-containing benzoxazine resin composition and application thereof

    CN117050463A

  • Bio-based benzoxazine monomer, resin and preparation method thereof

    CN117486822A

  • Preparation method of efficient flame-retardant phosphorus-containing benzoxazine epoxy resin copolymer

    CN117924637A

Cited By

  • Amine curing agent containing benzoxazine, epoxy resin composition and application thereof

    CN119955089A

  • Flame-retardant degradable main chain type benzoxazine and preparation method thereof

    CN122502653A

  • A flame-retardant degradable main chain type benzoxazine and a preparation method thereof

    CN122502653B