Preparation method of high-toughness EVA (Ethylene Vinyl Acetate) composite adhesive film
By using 1,3:2,4-dibenzyl sorbitol and nanohydrotalcite LDH in EVA composite film to form a β crystal structure, the problem of poor impact resistance of EVA composite film is solved. It significantly improves its impact toughness and mechanical properties, and extends the service life of photovoltaic modules.
Patent Information
- Application Number
- CN202411185624.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
The existing EVA composite adhesive films have insufficient mechanical properties and poor impact resistance, which are prone to damage when impacted, affecting the service cycle of photovoltaic modules.
Using a high toughness EVA composite film composed of EVA resin particles, POE particles, PMMA particles, composite toughening agents, silane coupling agents, antacids, anti-aging agents, ultraviolet absorbers, etc., through 1,3:2, 4-Dibenzene sorbitol and nanohydrotalcite LDH jointly toughen, forming a β-crystal structure, improving the toughness and strength of the film.
It significantly improves the impact toughness and mechanical properties of EVA photovoltaic adhesive film, reduces the chance of damage, and improves the mechanical strength and service performance of photovoltaic modules.
Smart Images

Figure BDA0005013405780000131
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photovoltaic adhesive films and relates to a method for preparing a high-toughness EVA composite adhesive film. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Photovoltaic cell encapsulation film (EVA) is a thermosetting adhesive film that is placed between glass backboards. Due to the superiority of EVA film in adhesion, durability, optical properties, etc., it is increasingly widely used in current components and various optical products. Chinese patent CN201610224522 discloses an EVA composite film with anti-PID performance: using 0.05-7% acrylamide cross-linking agent, 0.05-3% auxiliary cross-linking agent, 0.02-0.5% ultraviolet light stabilizer, 0.02-0.5% auxiliary antioxidant, 0.02-0.5% tackifier, conventional additives and the remainder EVA, by adjusting the EVA formula and improving the structure, the EVA composite film has high anti-PID performance.
[0004] However, the mechanical properties of the film are not ideal, and it is easy to cause impact damage and breakage when impacted. The film has poor impact resistance. Under the action of external forces, the photovoltaic modules are more easily damaged, and the service life of the photovoltaic modules is reduced.
[0005] The paper "Structural Regulation and Mechanical Toughening of PP / EVA / LDH Ternary Nanocomposites" disclosed the problem that the impact performance of PP / EVA / LDH materials is still poor. By introducing calcium pimelate (CaHA) in the β-nucleating agent and forming a synergistic toughening agent with LDH, the effects of CaHA and LDH on the morphology, structure and macroscopic properties of PP composites under different ratio parameters were systematically studied, and the optimal filler ratio was obtained through impact performance testing. However, the composite toughening agent composed of CaHA and LDH has a poor toughening modification effect on EVA / POE / PMM. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a highly transparent EVA composite film with high toughness while maintaining other mechanical properties of the film. The present invention solves the problem of poor mechanical impact resistance and insufficient mechanical strength of photovoltaic films.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The first aspect of the present invention provides a high-toughness EVA composite adhesive film, which is composed of the following raw materials in parts by weight: 75-85 parts of EVA resin particles, 0.3-5 parts of POE particles, 10-25 parts of PMMA particles, 0.2-2 parts of composite toughening agent, 0.1-0.5 parts of silane coupling agent, 0.1-4 parts of compatibilizer, 1-3 parts of antacid, 0.03 parts-0.3 parts of cross-linking agent, 0.5-2 parts of initiator, 0.1-2 parts of anti-aging agent, and 0.1-1 parts of ultraviolet absorber.
[0009] The composite toughening agent is a mixture of nano hydrotalcite and 1,3:2,4-dibenzylidene sorbitol, and the mass ratio of the two is 1:3-10. In the toughening agent of the present invention, 1,3:2,4-dibenzylidene sorbitol is used as a core agent, and its unique double benzene ring special structure interacts with EVA molecules to more easily induce the formation of a β-crystalline structure, which significantly improves the toughening and modification effect of EVA / POE / PMM. In the present invention, 1,3:2,4-dibenzylidene sorbitol and hydrotalcite LDH synergistically toughen, significantly improving the toughness and strength of the film.
[0010] In some embodiments, the initiator is at least one of tert-butyl isopropyl peroxycarbonate, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, tert-butyl peroxycarbonate-2-ethylhexyl ester, 1,1-di-tert-butyl peroxy-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0011] In some embodiments, the crosslinking agent is selected from at least one of trimethylolpropane trimethacrylate, hexanediol dimethacrylate, butanediol dimethacrylate, and ethylene glycol dimethacrylate.
[0012] In some embodiments, the antacid is dimethylaminomethyl acrylate.
[0013] In some embodiments, the compatibilizer is ethylene-co-glycidyl methacrylate.
[0014] In some embodiments, the antioxidant is tris[2,4-di-tert-butylphenyl]phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], or a mixture thereof.
[0015] In some embodiments, the ultraviolet absorber is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole, phenyl o-hydroxybenzoate, or a mixture of tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite and phenyl o-hydroxybenzoate.
[0016] In some embodiments, the silane coupling agent is KH 570.
[0017] The second aspect of the present invention provides a method for preparing a high-toughness EVA composite film, comprising:
[0018] The PMMA particles, the compatibilizer and the initiator are uniformly mixed to obtain a mixture, and then the mixture is fed into a twin-screw extruder, melt-extruded, cooled and pelletized to obtain modified PMMA-g-EGMA particles;
[0019] The modified PMMA-g-EGMA particles, EVA resin particles, POE particles, silane coupling agent, composite toughening agent, crosslinking agent, antacid, anti-aging agent and ultraviolet absorber are uniformly mixed, and the mixture is added to an extruder for mixing and plasticizing, melt extrusion, casting into a film, cutting and winding to obtain the product.
[0020] In some embodiments, the screw speed is set at 300-400 r / min, and the heating temperature is 200-300°C.
[0021] In some embodiments, the melting and refining temperature is set at 180°C-270°C.
[0022] More specifically, they include:
[0023] (1) adding PMMA particles, composite toughening agent and initiator into a high-speed mixer, setting the speed of the high-speed mixer to 1500-2500 r / min, mixing time to 30-40 min, then feeding the mixture into a twin-screw extruder, setting the screw speed to 300-400 r / min, heating temperature to 200-300° C., melt extruding, cooling and pelletizing to obtain modified PMMA-g-EGMA particles;
[0024] (2) Take the modified particles, EVA-g-MAH particles, POE particles, composite toughening agent, antacid, antioxidant, and ultraviolet absorber in proportion and add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticizing, melt extrusion, cast film, and cut and roll. The speed of the high-speed mixer is set to 1000-3000r / min, the mixing time is set to 10-30min, and the melting and refining temperature is set to between 180℃ and 270℃.
[0025] The third aspect of the present invention provides the use of the above-mentioned high-toughness EVA composite film in the preparation of photovoltaic modules.
[0026] Beneficial effects of the present invention
[0027] (1) The present invention adds 1,3:2,4-dibenzylidene sorbitol and hydrotalcite LDH to synergistically toughen the EVA composite film, thereby improving the crystallinity of EVA, so that the EVA photovoltaic film has high impact toughness and strong mechanical properties, and reduces the probability of breakage.
[0028] (2) The high-toughness photovoltaic composite film of the present invention has high impact resistance, which can effectively improve the mechanical strength of photovoltaic modules, reduce the probability of damage to the film under external force, and improve the performance.
[0029] (3) The preparation method of the present invention is simple, practical and easy to promote. DETAILED DESCRIPTION
[0030] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0031] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are intended to explain the present invention rather than to limit it.
[0032] Example 1
[0033] A high-toughness EVA composite film is composed of the following raw materials in parts by weight: 85 parts of EVA particles, 5 parts of POE particles, 8 parts of PMMA particles, 2 parts of composite toughening agent, 0.3 parts of silane coupling agent KH570, 0.8 parts of antacid, 0.1 parts of cross-linking agent, 0.1 parts of compatibilizer, 0.3 parts of initiator, 0.2 parts of anti-aging agent, and 0.1 parts of ultraviolet absorber; wherein the composite toughening agent is 1,3:2,4-dibenzylidene sorbitol and nano-hydrotalcite LDH (double metal hydroxide The antacid is dimethylaminomethyl acrylate, the compatibilizer is ethylene-glycidyl methacrylate copolymer (EGMA); the crosslinking agent is trimethylolpropane trimethacrylate; the initiator is dicumyl peroxide (DCP); the anti-aging agent is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; the ultraviolet absorber is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole;
[0034] The method for preparing the high-toughness EVA composite film of this embodiment is:
[0035] (1) adding PMMA particles, a compatibilizer, and an initiator into a high-speed mixer, setting the speed of the high-speed mixer to 2500 r / min, and mixing for 30 min, and then feeding the mixture into a twin-screw extruder, setting the screw speed to 400 r / min, heating the mixture to 300° C., and then pelletizing the mixture after cooling and melt extrusion to obtain modified PMMA-g-EGMA particles;
[0036] (2) Take the modified PMMA-g-EGMA particles, EVA particles, POE particles, composite toughening agent, antacid, antioxidant, UV absorber, crosslinking agent, and silane coupling agent according to the proportion, add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticizing, melt extrusion, cast film, and cut and roll. The speed of the high-speed mixer is set to 1500r / min, the mixing time is set to 20min, and the melting and refining temperature is set between 250°C.
[0037] Example 2
[0038] A high-toughness EVA composite material, composed of the following raw materials in parts by weight: 90 parts of EVA particles, 4 parts of POE particles, 5 parts of PMMA particles, 1.5 parts of a composite toughening agent, 0.3 parts of a silane coupling agent KH570, 0.5 parts of an antacid, 0.1 parts of a crosslinking agent, 0.2 parts of a compatibilizer, 0.3 parts of an initiator, 0.2 parts of an anti-aging agent, and 0.1 parts of an ultraviolet absorber; wherein the composite toughening agent is a mixture of 1,3:2,4-dibenzylidene sorbitol and LDH in a mass ratio of 1:7; the antacid is dimethylaminomethyl acrylate, and the The compatibilizer is ethylene-glycidyl methacrylate copolymer (EGMA); the crosslinker is hexanediol dimethacrylate; the initiator is 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane; the anti-aging agent is a 1:3 mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and tris[2,4-, di-tert-butylphenyl]phosphite; the ultraviolet absorber is a 1:1 mixture of tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite and phenyl o-hydroxybenzoate;
[0039] The method for preparing the high-toughness EVA composite film of this embodiment is:
[0040] (1) adding PMMA particles, a compatibilizer, and an initiator into a high-speed mixer, setting the speed of the high-speed mixer to 2000 r / min, and mixing for 45 min, and then feeding the mixture into a twin-screw extruder, setting the screw speed to 300 r / min, and heating the mixture to 270° C., and then pelletizing the mixture after melt extrusion, cooling, and obtaining modified PMMA-g-EGMA particles;
[0041] (2) Take the modified PMMA-g-EGMA particles, EVA particles, POE particles, composite toughening agent, antacid, antioxidant, UV absorber, crosslinking agent, and silane coupling agent according to the proportion, add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticizing, melt extrusion, cast film, and cut and roll. The speed of the high-speed mixer is set to 2000r / min, the mixing time is set to 30min, and the melting and refining temperature is set to 220℃.
[0042] Example 3
[0043] A high-toughness EVA composite material for photovoltaic adhesive film, composed of the following raw materials in parts by weight: 95 parts of EVA particles, 2 parts of POE particles, 2 parts of PMMA particles, 1 part of a composite toughening agent, 0.3 parts of a silane coupling agent KH570, 0.7 parts of an antacid, 0.05 parts of a cross-linking agent, 0.2 parts of a compatibilizer, 0.2 parts of an initiator, 0.1 parts of an anti-aging agent, and 0.1 parts of an ultraviolet absorber; wherein the composite toughening agent is a mixture of a β toughening agent and LDH in a mass ratio of 1:5; the antacid is dimethylaminomethyl acrylate, the compatibilizer The crosslinking agent is ethylene-glycidyl methacrylate copolymer (EGMA); the crosslinking agent is hexanediol dimethacrylate; the initiator is 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane; the anti-aging agent is a 1:3 mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and tris[2,4-, di-tert-butylphenyl]phosphite; the ultraviolet absorber is a 1:1 mixture of tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite and phenyl o-hydroxybenzoate;
[0044] The method for preparing the high-toughness EVA composite film of this embodiment is:
[0045] (1) adding PMMA particles, a compatibilizer, and an initiator into a high-speed mixer, setting the speed of the high-speed mixer to 1500 r / min, and mixing for 30 min, and then feeding the mixture into a twin-screw extruder, setting the screw speed to 300 r / min, and heating the mixture to 230° C., and then pelletizing the mixture after melt extrusion, cooling, and obtaining modified PMMA-g-EGMA particles;
[0046] (2) Take the modified PMMA-g-EGMA particles, EVA particles, POE particles, composite toughening agent, antacid, antioxidant, UV absorber, crosslinking agent, and silane coupling agent according to the proportion, add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticization, melt extrusion, cast film, and cut and roll. The speed of the high-speed mixer is set to 1500r / min, the mixing time is set to 35min, and the melting and refining temperature is set to 210℃.
[0047] Example 4
[0048] A high-toughness EVA composite material for photovoltaic adhesive film, composed of the following raw materials in parts by weight: 87 parts of EVA particles, 3 parts of POE particles, 1 part of PMMA particles, 1.8 parts of composite toughening agent, 0.3 parts of silane coupling agent KH570, 0.3 parts of antacid, 0.15 parts of crosslinking agent, 0.15 parts of compatibilizer, 0.15 parts of initiator, 0.2 parts of anti-aging agent, 0.1 parts of ultraviolet absorber; wherein the composite toughening agent is a mixture of 1,3:2,4-dibenzylidene sorbitol and nano-hydrotalcite LDH (double metal hydroxide) in a mass ratio of 1:5; the antacid is Dimethylaminomethyl acrylate, the compatibilizer is ethylene-glycidyl methacrylate copolymer (EGMA); the crosslinker is hexanediol dimethacrylate; the initiator is 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane; the anti-aging agent is a 1:3 mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and tris[2,4-, di-tert-butylphenyl]phosphite; the ultraviolet absorber is a 1:1 mixture of tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite and phenyl o-hydroxybenzoate;
[0049] The method for preparing the high-toughness EVA composite film of this embodiment is:
[0050] (1) adding PMMA particles, a compatibilizer, and an initiator into a high-speed mixer, setting the speed of the high-speed mixer to 2000 r / min, and mixing for 30 min, and then feeding the mixture into a twin-screw extruder, setting the screw speed to 400 r / min, heating the mixture to 200° C., and then pelletizing the mixture after cooling and melt extrusion to obtain modified PMMA-g-EGMA particles;
[0051] (2) Take the modified PMMA-g-EGMA particles, EVA particles, POE particles, composite toughening agent, antacid, antioxidant, UV absorber, crosslinking agent, and silane coupling agent according to the proportion, add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticization, melt extrusion, cast film, and cut and roll. The speed of the high-speed mixer is set to 2200r / min, the mixing time is set to 30min, and the melting and refining temperature is set to 250°C.
[0052] Example 5
[0053] A high-toughness EVA composite material for photovoltaic adhesive film, composed of the following raw materials in parts by weight: 87 parts of EVA particles, 3 parts of POE particles, 1 part of PMMA particles, 1.8 parts of composite toughening agent, 0.3 parts of silane coupling agent KH570, 0.3 parts of antacid, 0.15 parts of cross-linking agent, 0.15 parts of compatibilizer, 0.15 parts of initiator, 0.2 parts of anti-aging agent, and 0.1 parts of ultraviolet absorber; wherein the composite toughening agent is a mixture of 1,3:2,4-dibenzylidene sorbitol and nano-hydrotalcite LDH (double metal hydroxide) in a mass ratio of 1:3; the compatibilizer is ethylene-glycidyl methacrylate copolymer (EGMA); the cross-linking agent is ethylene glycol dimethacrylate; the initiator is dicyclohexyl peroxydicarbonate; the anti-aging agent is tris[2,4-di-tert-butylphenyl]phosphite; the ultraviolet absorber is phenyl o-hydroxybenzoate;
[0054] The method for preparing the high-toughness EVA composite film of this embodiment is:
[0055] (1) adding PMMA particles, a compatibilizer, and an initiator into a high-speed mixer, setting the speed of the high-speed mixer to 2000 r / min, and mixing for 45 min, and then feeding the mixture into a twin-screw extruder, setting the screw speed to 400 r / min, and heating the mixture to 230° C., and then pelletizing the mixture after cooling and melt extrusion to obtain modified PMMA-g-EGMA particles;
[0056] (2) Take the modified PMMA-g-EGMA particles, EVA particles, POE particles, composite toughening agent, antacid, antioxidant, UV absorber, crosslinking agent, silane coupling agent KH-570 according to the proportion, add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticization, melt extrusion, cast film, cut and roll. The speed of the high-speed mixer is set to 3000r / min, the mixing time is set to 45min, and the melting and refining temperature is set to 250°C.
[0057] Comparative Example 1
[0058] In step (2), the raw materials do not contain a composite toughening agent, and the rest is the same as in Example 1. The details are as follows:
[0059] A high-toughness EVA composite adhesive film material is composed of the following raw materials in parts by weight: 85 parts of EVA particles, 5 parts of POE particles, 8 parts of PMMA particles, 0 parts of composite toughening agent, 0.3 parts of silane coupling agent KH-570, 0.8 parts of antacid, 0.1 parts of cross-linking agent, 0.1 parts of compatibilizer, 0.3 parts of initiator, 0.2 parts of anti-aging agent, and 0.1 parts of ultraviolet absorber; the antacid is dimethylaminomethyl acrylate, and the compatibilizer is ethylene-glycidyl methacrylate copolymer (EGMA); the cross-linking agent is trimethylolpropane trimethacrylate; the initiator is diisopropylbenzene peroxide (DCP); the anti-aging agent is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; the ultraviolet absorber is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole;
[0060] The method for preparing the high-toughness EVA composite film of this comparative example is:
[0061] (1) adding PMMA particles, a compatibilizer, and an initiator into a high-speed mixer, setting the speed of the high-speed mixer to 2500 r / min, and mixing for 30 min, and then feeding the mixture into a twin-screw extruder, setting the screw speed to 400 r / min, heating the mixture to 300° C., and then pelletizing the mixture after cooling and melt extrusion to obtain modified PMMA-g-EGMA particles;
[0062] (2) Take the modified PMMA-g-EGMA particles, EVA particles, POE particles, antacid, antioxidant, UV absorber, crosslinking agent, silane coupling agent KH-570 according to the proportion, add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticization, melt extrusion, cast film, cut and roll. The speed of the high-speed mixer is set to 1500r / min, the mixing time is set to 20min, and the melting and refining temperature is set between 250℃.
[0063] Comparative Example 2
[0064] In step (2), only nano-hydrotalcite is added as the toughening agent in the raw materials, and the rest is the same as in Example 1. The details are as follows:
[0065] A high-toughness EVA composite adhesive film material is composed of the following raw materials in parts by weight: 85 parts of EVA particles, 5 parts of POE particles, 8 parts of PMMA particles, 2 parts of nano-hydrotalcite as a toughening agent, 0.3 parts of silane coupling agent KH-570, 0.8 parts of antacid, 0.1 parts of cross-linking agent, 0.1 parts of compatibilizer, 0.3 parts of initiator, 0.2 parts of anti-aging agent, and 0.1 parts of ultraviolet absorber; the antacid is dimethylaminomethyl acrylate, and the compatibilizer is ethylene-glycidyl methacrylate copolymer (EGMA); the cross-linking agent is trimethylolpropane trimethacrylate; the initiator is diisopropylbenzene peroxide (DCP); the anti-aging agent is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; the ultraviolet absorber is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole;
[0066] The method for preparing the high-toughness EVA composite film of this comparative example is:
[0067] (1) adding PMMA particles, a compatibilizer, and an initiator into a high-speed mixer, setting the speed of the high-speed mixer to 2500 r / min, and mixing for 30 min, and then feeding the mixture into a twin-screw extruder, setting the screw speed to 400 r / min, heating the mixture to 300° C., and then pelletizing the mixture after cooling and melt extrusion to obtain modified PMMA-g-EGMA particles;
[0068] (2) Take the modified PMMA-g-EGMA particles, EVA particles, POE particles, nano-hydrotalcite, antacid, antioxidant, UV absorber, crosslinking agent, silane coupling agent KH-570 according to the proportion, add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticizing, melt extrusion, cast film, cut and roll. The speed of the high-speed mixer is set to 1500r / min, the mixing time is set to 20min, and the melting and refining temperature is set between 250°C.
[0069] Comparative Example 3
[0070] In step (2), only 1,3:2,4-dibenzylidene sorbitol is added as the toughening agent in the raw materials, and the rest is the same as in Example 1. The details are as follows:
[0071] A high-toughness EVA composite adhesive film material is composed of the following raw materials in parts by weight: 85 parts of EVA particles, 5 parts of POE particles, 8 parts of PMMA particles, 2 parts of 1,3:2,4-dibenzylidene sorbitol, 0.3 parts of silane coupling agent KH-570, 0.8 parts of antacid, 0.1 parts of cross-linking agent, 0.1 parts of compatibilizer, 0.3 parts of initiator, 0.2 parts of anti-aging agent, and 0.1 parts of ultraviolet absorber; the antacid is dimethylaminomethyl acrylate, and the compatibilizer is ethylene-glycidyl methacrylate copolymer (EGMA); the cross-linking agent is trimethylolpropane trimethacrylate; the initiator is diisopropyl peroxide (DCP); the anti-aging agent is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; the ultraviolet absorber is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole;
[0072] The method for preparing the high-toughness EVA composite film of this comparative example is:
[0073] (1) adding PMMA particles, a compatibilizer, and an initiator into a high-speed mixer, setting the speed of the high-speed mixer to 2500 r / min, and mixing for 30 min, and then feeding the mixture into a twin-screw extruder, setting the screw speed to 400 r / min, heating the mixture to 300° C., and then pelletizing the mixture after cooling and melt extrusion to obtain modified PMMA-g-EGMA particles;
[0074] (2) Take the modified PMMA-g-EGMA particles, EVA particles, POE particles, 1,3:2,4-dibenzylidene sorbitol, antacid, antioxidant, UV absorber, crosslinking agent, and silane coupling agent according to the proportion, add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticizing, melt extrusion, cast film, and cut and roll. The speed of the high-speed mixer is set to 1500r / min, the mixing time is set to 20min, and the melting and refining temperature is set between 250°C.
[0075] Comparative Example 4
[0076] The composite toughening agent in the raw material of step (2) is a mixture of calcium pimelate and nano-hydrotalcite LDH (double metal hydroxide) in a mass ratio of 1:10, and the rest is the same as in Example 1. The details are as follows:
[0077] A high-toughness EVA composite adhesive film material is composed of the following raw materials in parts by weight: 85 parts of EVA particles, 5 parts of POE particles, 8 parts of PMMA particles, 2 parts of composite toughening agent, 0.3 parts of silane coupling agent KH-570, 0.8 parts of antacid, 0.1 parts of cross-linking agent, 0.1 parts of compatibilizer, 0.3 parts of initiator, 0.2 parts of anti-aging agent, and 0.1 parts of ultraviolet absorber; the antacid is dimethylaminomethyl acrylate, and the compatibilizer is ethylene-glycidyl methacrylate copolymer (EGMA); the cross-linking agent is trimethylolpropane trimethacrylate; the initiator is dicumyl peroxide (DCP); the anti-aging agent is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; the ultraviolet absorber is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole;
[0078] The method for preparing the high-toughness EVA composite film of this comparative example is:
[0079] (1) adding PMMA particles, a compatibilizer, and an initiator into a high-speed mixer, setting the speed of the high-speed mixer to 2500 r / min, and mixing for 30 min, and then feeding the mixture into a twin-screw extruder, setting the screw speed to 400 r / min, heating the mixture to 300° C., and then pelletizing the mixture after cooling and melt extrusion to obtain modified PMMA-g-EGMA particles;
[0080] (2) Take the modified PMMA-g-EGMA particles, EVA particles, POE particles, composite toughening agent, antacid, antioxidant, UV absorber, crosslinking agent, and silane coupling agent according to the proportion, add them to the high-speed stirring and mix them evenly, add the mixture to the extruder for mixing and plasticizing, melt extrusion, cast film, and cut and roll. The speed of the high-speed mixer is set to 1500r / min, the mixing time is set to 20min, and the melting and refining temperature is set between 250°C.
[0081] Test experiment:
[0082] Referring to the standard GB / T29848-2018 "Ethylene-vinyl acetate copolymer (EVA) film for photovoltaic module encapsulation", the performance tests were carried out on the film samples prepared in Examples 1-5 and Comparative Example 1. The thickness of the film samples was 400 μm. The specific test results are shown in Table 1.
[0083] Table 1
[0084]
[0085] From the comparison between Example 1 and Comparative Example 1, it can be seen that the addition of the composite toughening agent effectively improves the impact resistance and mechanical strength of the film.
[0086] From the comparison between Example 1 and Comparative Examples 2 and 3, it can be seen that, compared with adding 1,3:2,4-dibenzylidene sorbitol or nano-hydrotalcite LDH (double metal hydroxide) alone, the combination of the two can better improve the impact resistance and mechanical strength of the film.
[0087] From the comparison between Example 1 and Comparative Example 4, it can be seen that compared with the composite toughening agent composed of CaHA and LDH, the composite toughening agent composed of 1,3:2,4-dibenzylidene sorbitol and nano-hydrotalcite LDH (double metal hydroxide) can better improve the mechanical strength of the EVA composite film.
[0088] In summary, the high-toughness photovoltaic composite film in the present invention has high impact resistance, can effectively improve the mechanical strength of photovoltaic modules, reduce the probability of damage to the film under external forces, and improve the performance.
[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-toughness EVA composite film, characterized in that: The invention is composed of the following raw materials in parts by weight: 75-85 parts of EVA resin particles, 0.3-5 parts of POE particles, 10-25 parts of PMMA particles, 0.2-2 parts of composite toughening agent, 0.1-0.5 parts of silane coupling agent, 0.1-4 parts of compatibilizer, 1-3 parts of antacid, 0.03-0.3 parts of crosslinking agent, 0.5-2 parts of initiator, 0.1-2 parts of anti-aging agent and 0.1-1 parts of ultraviolet absorber; The composite toughening agent is prepared by mixing nano hydrotalcite and 1,3:2,4-dibenzylidene sorbitol, and the mass ratio of the two is 1:3-10.
2. The high-toughness EVA composite film according to claim 1, characterized in that: The initiator is at least one of tert-butyl isopropyl peroxycarbonate, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, tert-butyl peroxycarbonate-2-ethylhexyl ester, 1,1-di-tert-butyl peroxy-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butyl peroxy)hexane, and 2,5-dimethyl-2,5-di(tert-butyl peroxy)hexane.
3. The high-toughness EVA composite film according to claim 1, characterized in that: The crosslinking agent is selected from at least one of trimethylolpropane trimethacrylate, hexanediol dimethacrylate, butanediol dimethacrylate and ethylene glycol dimethacrylate.
4. The high-toughness EVA composite film according to claim 1, characterized in that: The antacid is dimethylaminomethyl acrylate.
5. The high-toughness EVA composite film according to claim 1, characterized in that: The compatibilizer is ethylene-glycidyl methacrylate copolymer; Alternatively, the antioxidant is tris[2,4-di-tert-butylphenyl]phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], or a mixture thereof.
6. The high-toughness EVA composite film according to claim 1, characterized in that: The ultraviolet absorber is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole, phenyl o-hydroxybenzoate, or a mixture of tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite and phenyl o-hydroxybenzoate.
7. A method for preparing a high-toughness EVA composite film, characterized in that: include: The PMMA particles, the compatibilizer and the initiator are uniformly mixed to obtain a mixture, and then the mixture is fed into a twin-screw extruder, melt-extruded, cooled and pelletized to obtain modified PMMA-g-EGMA particles; The modified PMMA-g-EGMA particles, EVA resin particles, POE particles, silane coupling agent, composite toughening agent, crosslinking agent, antacid, anti-aging agent and ultraviolet absorber are uniformly mixed, and the mixture is added to an extruder for mixing and plasticizing, melt extrusion, casting into a film, cutting and winding to obtain the product.
8. The method for preparing the high-toughness EVA composite film according to claim 7, characterized in that: The screw speed is set at 300-400r / min, and the heating temperature is 200-300°C.
9. The method for preparing the high-toughness EVA composite film according to claim 7, characterized in that: The melting and refining temperature is set at 180°C-270°C.
10. Use of the high-toughness EVA composite film according to any one of claims 1 to 9 in the preparation of photovoltaic modules.
Citation Information
Cited By
Long-acting anti-freezing photovoltaic adhesive film, preparation method thereof and photovoltaic module
CN122521254A