Absorbable copolymer as well as preparation method and application thereof
Through the step-by-step copolymerization technology of glycolide, lactide and trimethylene carbonate, PGLT copolymer is formed, which solves the shortcomings of existing materials in terms of mechanical properties and degradation speed, and achieves high mechanical properties and suitable degradation time. Absorbable tissue-closing clip material, suitable for medical devices.
Patent Information
- Application Number
- CN202411050136.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing absorbable tissue closure clip materials have shortcomings in terms of mechanical properties, rigid strength and degradation speed, and it is difficult to meet the needs of medical devices at the same time.
Glycolide, lactide and trimethylene carbonate are used to form PGLT copolymers through step-by-step copolymerization, and the proportion of each chain segment is adjusted to improve the toughness and degradation properties of the material, forming high mechanical strength, flexibility and suitable degradation time. absorbable copolymer.
The prepared PGLT copolymer has suitable mechanical properties and degradation time. It is suitable for the preparation of medical devices such as absorbable tissue closed clips, improving the toughness and degradation properties of the material and extending the service life.
Smart Images

Figure CN118978678A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical devices, and in particular relates to an absorbable copolymer and a preparation method and application thereof. Background Art
[0002] Tissue closure clips are commonly used in minimally invasive laparoscopic surgery, mainly used to clamp on duct tissues, among which the tissue closure clips with V-shaped lock structure have the best effect. Tissue closure clips are divided into absorbable closure clips and non-absorbable closure clips according to whether they can be degraded in the body. Non-absorbable closure clips are made of metal or non-degradable polymer materials. Non-absorbable closure clips cannot be absorbed by the human body, which greatly limits their clinical application.
[0003] The absorbable closure clip (Absolok Extra, US4424810) developed by Johnson & Johnson of the United States has a V-shaped locking structure and is made of absorbable polydioxanone PPDO. This material has good softness but low strength, so the clamping force is insufficient. During use, it will deform and cause the clamped tissue to slip or jump out of the clamp. When there is omentum tissue around the duct tissue in the body, it is difficult to penetrate the omentum tissue to achieve closure.
[0004] Among the degradable and absorbable materials, PGA (polyglycolic acid or polyglycolide) has high mechanical strength, high rigidity, and good crystallinity, but lacks toughness and degrades quickly, making it difficult to use as a V-shaped clamp with large forces. Therefore, blending is usually used to improve the toughness of degradable polymer materials, such as blending PGA with softer materials such as polydioxanone (PPDO), polytrimethylene carbonate (PTMC), and polycaprolactone (PCL) to improve the toughness of the material. However, due to compatibility issues, the composite material degrades faster and cannot meet the requirements of closed clamp materials.
[0005] Although copolymerization can improve the toughness of biodegradable polymer materials GA, the formation of random copolymers will reduce the crystallinity of GA segments, resulting in reduced mechanical strength and faster degradation than GA polymers. Step-by-step block copolymerization can also increase the toughness of PGA materials, that is, the tough monomer is polymerized into a prepolymer as a soft segment, and then copolymerized with GA monomer to form a hard segment. However, the material formed by this polymerization method is difficult to control. When the material is soft, it is only suitable for sutures. If the strength is increased by increasing the GA content in the hard segment, the degradation rate will increase.
[0006] In summary, whether it is the method of blending or copolymerization to toughen PGA, it cannot solve the problems of mechanical properties and degradation rate at the same time. Therefore, the research of degradable and absorbable medical materials with excellent mechanical properties, rigidity and degradation rate is a hot topic in the field of medical device manufacturing. Summary of the invention
[0007] The present invention is to solve the above problems and provides an absorbable copolymer and a preparation method and application thereof.
[0008] The present invention adopts the following technical scheme: a method for preparing an absorbable copolymer, wherein a PGLT copolymer is formed by step-by-step copolymerization of glycolide, lactide and trimethylene carbonate, wherein the weight percentage of glycolide in the PGLT copolymer is 60%-85%, the weight percentage of lactide is 5%-25%, and the weight percentage of trimethylene carbonate is 8%-25%. In the step-by-step copolymerization process, lactide and trimethylene carbonate are first polymerized into a prepolymer and then copolymerized with glycolide. The PGLT copolymer contains three chain segments of polymerized glycolide, polymerized lactide and polymerized trimethylene carbonate, and specifically comprises the following steps:
[0009] (1) Reactant A: lactide or lactide and glycolide are polymerized in the presence of an initiator and a catalyst to form a homopolymer or a copolymer;
[0010] (2) reactant B: trimethylene carbonate or trimethylene carbonate and glycolide are polymerized in the presence of an initiator and a catalyst to form a homopolymer or a copolymer;
[0011] (3) Copolymerization: glycolide is used as reactant C. Reactant C is melt-blended with reactants B and A and polymerized in an air-tight reactor to form a PGLT copolymer.
[0012] Further, a method for preparing an absorbable copolymer comprises:
[0013] (1) Reactant A: Add 0.01%-0.2% by weight of an initiator and 0.01%-0.1% by weight of a catalyst, add lactide and glycolide to a reactor under nitrogen protection or vacuum conditions, raise the temperature to 150° C.-180° C., maintain the reaction temperature for 6-15 hours, and perform ring-opening polymerization to obtain reactant A;
[0014] (2) Reactant B: add 0.01%-0.2% by weight of an initiator and 0.01%-0.1% by weight of a catalyst, add trimethylene carbonate and glycolide to the reactor under nitrogen protection or vacuum conditions, raise the temperature to 150° C.-180° C., maintain the reaction temperature for 2-8 hours, and perform ring-opening polymerization to obtain reactant B;
[0015] (3) Copolymerization: With glycolide as reactant C, reactant C is melt-blended with reactants A and B, and polymerized at 200°C-230°C in an air-isolated reactor to form a PGLT copolymer containing glycolide, lactide and trimethylene carbonate.
[0016] Furthermore, the initiator is a monohydric alcohol, a dihydric alcohol or a polyhydric alcohol among fatty alcohols, and the catalyst is stannous octoate.
[0017] Furthermore, the lactide is one or more of L-lactide, DL-lactide or D-lactide.
[0018] Further, in reactant A, the weight percentage of glycolide is 0-20%, and in reactant B, the weight percentage of glycolide is 0-20%.
[0019] The proportion of glycolide, lactide, and trimethylene carbonate in the PGLT copolymer in the present invention is the best solution obtained by designing and adjusting the mechanical strength, hardness (or toughness), and degradation time of the copolymer according to the material requirements of the absorbable closure clip. Too high a lactide content in the PGLT copolymer is not good for the mechanical properties, such as stress relaxation during the use of the closure clip, which may cause the clamped pipe to loosen, and too low a content will affect the degradation performance of the copolymer; too high a trimethylene carbonate content will reduce its mechanical properties, and too low a content will reduce the flexibility of the copolymer; too high a glycolide content will cause the copolymer to degrade faster and its toughness will deteriorate, and too low a content will reduce the mechanical properties of the copolymer.
[0020] The elastic modulus of the prepared absorbable copolymer is 600MPa-2300MPa, the tensile yield strength is greater than 40MPa, and the tensile elongation at break is not less than 40%.
[0021] Furthermore, the elastic modulus of the PGLT copolymer is 800MPa-2000MPa, the tensile yield strength is greater than 50MPa, and the tensile elongation at break is not less than 50%.
[0022] Furthermore, the intrinsic viscosity of the PGLT copolymer measured in hexafluoroisopropanol at a concentration of 0.1 g / dl at 25° C. is 0.8-2.5 dl / g.
[0023] Furthermore, the PGLT copolymer has a tensile strength of not less than 5 MPa after being immersed in a phosphate buffer solution at 37° C. for 14 days.
[0024] The invention discloses an application of an absorbable copolymer, wherein the absorbable copolymer can be used to prepare a tissue closure clip, a suture clip, a suture anchor, an anastomosis staple, a surgical suture, a puncture plugger or an anal fistula plugger.
[0025] The PGLT copolymer of the present invention comprises three reactants: reactant A, reactant B and reactant C in various combinations, including: A-C+B+C, ACB, ABC, CAB, CAC, CBC, CABC, etc. The structural formula of ABC is shown in the figure:
[0026]
[0027] Compared with random copolymers, the PGLT copolymer of the present invention fully demonstrates the characteristics of each segment of reactant A, reactant B and reactant C. Compared with the large amount of random polymerization between GA monomer and LA monomer in the existing polymer, the present invention uses a step-by-step copolymerization method to form a lactide segment, a trimethylene carbonate segment and a glycolide copolymerized by prepolymerization, without a greater change due to copolymerization, thereby avoiding the problem that the crystallinity cannot be improved after LA is doped in the GA chain formed by a large amount of random copolymerization between GA monomer and LA monomer, and the material strength after copolymerization is low and the degradation rate is fast; the segment formed by the polymerization of glycolide of reactant C has high crystallinity as a hard segment, which determines the high mechanical strength of the copolymer; the lactide segment formed by reactant A has high mechanical strength and slow degradation as a hard segment, which mainly acts on the strength of the PGLT copolymer and slows down the degradation; the trimethylene carbonate segment formed by reactant B has flexibility and slow degradation as a soft segment, making the PGLT copolymer soft.
[0028] The PGLT copolymer prepared by the present invention can achieve control of the intrinsic viscosity range of the copolymer by the intrinsic viscosity of the reactant A and reactant B segments, wherein the intrinsic viscosity of the reactant A at 25°C in chloroform with a concentration of 0.1 g / dl is 1.0 to 4.0 dl / g; the intrinsic viscosity of the reactant B at 25°C in chloroform with a concentration of 0.1 g / dl is 1.0 to 4.0 dl / g.
[0029] The advantages of the present invention are specifically as follows:
[0030] (1) The preparation method of the present invention is simple and the steps are easy to operate. The copolymer is formed by a step-by-step copolymerization method. First, lactide and trimethylene carbonate are polymerized into a prepolymer and then copolymerized with glycolide to form a prepolymer, which greatly reduces the randomness during the copolymerization process.
[0031] (2) The copolymer prepared by the present invention is copolymerized from a soft segment prepolymer - trimethylene carbonate and its copolymer, a hard segment prepolymer - lactide and its copolymer, and glycolide GA. The copolymer retains the characteristics of each segment, which not only improves the toughness of the material, but also avoids the problem of accelerated degradation caused by excessive glycolide GA content. By adjusting the proportion of each reactant, the mechanical strength, toughness and degradation time of the copolymer can be regulated, and a polymer material suitable for absorbable medical devices such as absorbable closure clips is prepared, which has broad application prospects in the field of medical devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The absorbable copolymer of the present invention1 HNMR spectrum.
[0033] Figure 2 The DSC thermal analysis spectrum of the absorbable copolymer of the present invention is shown in FIG.
[0034] Figure 3 Schematic diagram of the structure of the V-shaped absorbable closure clip. DETAILED DESCRIPTION
[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the present invention is further explained and illustrated in conjunction with specific embodiments below.
[0036] Example 1
[0037] The preparation of glycolide, L-lactide, trimethylene carbonate PGLT copolymer 1 (PGLT1) comprises the following steps:
[0038] (1) Preparation of reactant A: 200 g of L-lactide monomer (LA) was placed in a 3 L stainless steel reactor, and 0.04 wt % of stannous octoate catalyst and 0.05 wt % of diethylene glycol were added. The system temperature was raised to 170° C. under nitrogen protection, and polymerization reaction was carried out for 9 hours to obtain reactant A, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 2.03 dl / g. The tensile strength of reactant A obtained by mechanical test at 25° C. was 64 MPa, and the elongation at break was 10%;
[0039] (2) Preparation of reactant B: 200 g of trimethylene carbonate monomer (TMC) was placed in a 3 L stainless steel reactor, and 0.04 wt % of stannous octoate catalyst and 0.05 wt % of diethylene glycol were added. The system temperature was raised to 180° C. under nitrogen protection, and polymerization reaction was carried out for 4 hours to obtain reactant B, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 1.56 dl / g. The tensile strength of reactant B obtained by mechanical test at 25° C. was 4 MPa, and the elongation at break was 421%;
[0040] (3) Preparation of PGLT1: 170 g of reactant A, 150 g of reactant B and 680 g of glycolide (GA) were added to a 3 L stainless steel reactor. Under nitrogen protection, the temperature was raised to 215°C and maintained for 4 hours to obtain PGLT1, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.45 dl / g.
[0041] Figure 1 For PGLT copolymer 1 HNMR spectrum. 1H NMR spectrum was used to determine the weight percentage of glycolide, L-lactide and trimethylene carbonate monomer components in PGLT1 copolymer. With deuterated trifluoroacetic acid as solvent, the characteristic peak a of the methylene group of glycolide polymer segment appeared at 4.8-5.3ppm, the characteristic peak b of the second methyl group of lactide polymer segment was between 5.3 and 5.5ppm, and the characteristic peak c of the methylene group adjacent to the oxygen atom in the trimethylene carbonate polymer segment was between 4.3 and 4.6ppm. Peak a0 represents the chemical shift of the methylene group of GA homopolymer segment, and peaks a1, a2, a3 and a4 represent the chemical shifts of the methylene group of the random segment formed by chemical reactions such as GA transesterification. Peak c0 represents the chemical shift of the methylene group adjacent to the oxygen atom of TMC homopolymer segment, and peaks c1 and c2 represent the chemical shifts of the methylene group adjacent to the oxygen atom of the random segment formed by chemical reactions such as TMC transesterification. In summary, the numbers of glycolide homopolymer segments, lactide homopolymer segments and trimethylene carbonate homopolymer segments are much larger than the random segments, which proves that the PGLT copolymer has been successfully synthesized.
[0042] like Figure 1 As shown, the respective proportions can be calculated by the integrated areas of the three peaks a, b, and c. The weight percentage of glycolide (Gw) is calculated by the following formula:
[0043]
[0044] a=a0+a1+a2+a3+a4;
[0045] By analogy, the weight percentages of L-lactide (Lw) and trimethylene carbonate (Tw) are calculated as follows:
[0046]
[0047] c=c0+c1+c2.
[0048] The G / L / T ratio (weight %) in the examples and comparative examples calculated using the above method is shown in Table 1.
[0049] The PGLT copolymer was injection molded at about 225°C to form a dumbbell with a thickness of 2 mm. The material was stretched at a speed of 10 mm / min on a universal mechanical testing machine to test the tensile yield strength and elongation at break. The tensile modulus was the slope of the straight line on the stress-strain curve at a speed of 1 mm / min, as shown in Table 1.
[0050] The crystallinity of the synthesized PGLT copolymer was tested by differential scanning calorimetry (DSC) at a heating rate of 10°C / min. Figure 2As shown, the crystallinity refers to the crystallinity (C) of the PGA segment in the PGLT copolymer. In the DSC graph, there will be a melting peak of the PGA segment at not less than 210°C. The melting heat endotherm value of the melting peak can be used to calculate the crystallinity. The calculation formula is as follows
[0051]
[0052] Wherein ΔH is the difference (J / g) between the melting heat endurance of the PGA segment in the DSC spectrum and its crystallization heat endurance (if any), 203 (J / g) is the melting heat endurance of completely crystallized GA (Lebedev BV, Yepstropov AA, Kiparisova VG, Belov BI. Polym Sci USSR 1978; 20:32), and w is the weight percentage of GA. The results are shown in Table 1.
[0053] Example 2
[0054] Preparation of glycolide, L-lactide, trimethylene carbonate PGLT copolymer 2 (PGLT2):
[0055] (1) Preparation of reactant A: 160 g of L-lactide (LA) and 40 g of glycolide (GA) were placed in a 3 L stainless steel reactor, and 0.03% by weight of stannous octoate catalyst and 0.06% by weight of diethylene glycol were added. The system temperature was raised to 180° C. under nitrogen protection, and polymerization reaction was carried out for 6 hours to obtain reactant A, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 1.88 dl / g. The tensile strength of reactant A obtained by mechanical test at 25° C. was 49 MPa, and the elongation at break was 10%;
[0056] (2) Preparation of reactant B: 200 g of trimethylene carbonate (TMC) and 40 g of glycolide (GA) were placed in a 3 L stainless steel reactor, and 0.02 wt % of stannous octoate catalyst and 0.08 wt % of diethylene glycol were added. The system temperature was raised to 170° C. under nitrogen protection, and polymerization reaction was carried out for 5 hours to obtain reactant B, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 1.50 dl / g. The tensile strength of reactant B obtained by mechanical test at 25° C. was 4 MPa, and the elongation at break was 402%;
[0057] (3) Preparation of PGLT2: 170 g of reactant A, 150 g of reactant B and 680 g of glycolide were added to a 3 L stainless steel reactor. Under nitrogen protection, the temperature was raised to 220°C and maintained for 3 hours to obtain PGLT2, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.30 dl / g.
[0058] The composition ratio determination and performance characterization of PGLT2 are the same as those in Example 1, see Table 1.
[0059] Example 3
[0060] The preparation of glycolide, L-lactide, trimethylene carbonate PGLT copolymer 3 (PGLT3) comprises the following steps:
[0061] (1) Preparation of reactant A: 180 g of L-lactide (LA) and 20 g of glycolide (GA) were placed in a 3 L stainless steel reactor, and 0.02% by weight of stannous octoate catalyst and 0.16% by weight of octadecyl alcohol were added. The system temperature was raised to 165° C. under nitrogen protection, and the polymerization reaction was carried out for 10 hours to obtain reactant A, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 2.48 dl / g. The tensile strength of reactant A obtained by mechanical test at 25° C. was 58 MPa, and the elongation at break was 10%;
[0062] (2) Preparation of reactant B: 180 g of trimethylene carbonate (TMC) and 20 g of glycolide (GA) were placed in a 3 L stainless steel reactor, and 0.02 wt % of stannous octoate catalyst and 0.16 wt % of octadecyl alcohol were added. The system temperature was raised to 170° C. under nitrogen protection, and the polymerization reaction was carried out for 5 hours to obtain reactant B, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 1.78 dl / g. The tensile strength of reactant B obtained by mechanical test at 25° C. was 5 MPa, and the elongation at break was 455%;
[0063] (3) Preparation of PGLT3: 200 g of reactant A, 150 g of reactant B and 650 g of glycolide were added to a 3 L stainless steel reactor. Under nitrogen protection, the temperature was raised to 220°C and maintained for 4 hours to obtain PGLT3, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.62 dl / g.
[0064] The composition ratio determination and performance characterization of PGLT3 are the same as those in Example 1, see Table 1.
[0065] Example 4
[0066] The preparation of glycolide, L-lactide, trimethylene carbonate PGLT copolymer 4 (PGLT4) comprises the following steps:
[0067] (1) Preparation of reactant A: 190 g of L-lactide (LA) and 10 g of glycolide (GA) were placed in a 3 L stainless steel reactor, and 0.01 wt % of stannous octoate catalyst and 0.03 wt % of diethylene glycol were added. The system temperature was raised to 165° C. under nitrogen protection, and the polymerization reaction was carried out for 12 hours to obtain reactant A, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 2.67 dl / g. The tensile strength of reactant A obtained by mechanical test at 25° C. was 60 MPa, and the elongation at break was 7%;
[0068] (2) Preparation of reactant B: 190 g of trimethylene carbonate (TMC) and 10 g of glycolide (GA) were placed in a 3 L stainless steel reactor, and 0.01 wt % of stannous octoate catalyst and 0.15 wt % of octadecyl alcohol were added. The system temperature was raised to 170° C. under nitrogen protection, and polymerization reaction was carried out for 6 hours to obtain reactant B, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 1.99 dl / g. The tensile strength of reactant B obtained by mechanical test at 25° C. was 5 MPa, and the elongation at break was 460%;
[0069] (3) Preparation of PGLT4: 150 g of reactant A, 100 g of reactant B and 750 g of glycolide were added to a 3 L stainless steel reactor. Under nitrogen protection, the temperature was raised to 220°C and maintained for 4 hours to obtain PGLT4, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.73 dl / g.
[0070] The composition ratio determination and performance characterization of PGLT4 are the same as those in Example 1, see Table 1.
[0071] Example 5
[0072] Preparation of glycolide, L-lactide, trimethylene carbonate PGLT copolymer 4 (PGLT5):
[0073] (1) Preparation of reactant A: 170 g of L-lactide (LA) and 30 g of glycolide (GA) were placed in a 3 L stainless steel reactor, and 0.01 wt % of stannous octoate catalyst and 0.13 wt % of dodecanol were added. The system temperature was raised to 165° C. under nitrogen protection, and the polymerization reaction was carried out for 12 hours to obtain reactant A, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 2.24 dl / g. The tensile strength of reactant A obtained by mechanical test at 25° C. was 48 MPa, and the elongation at break was 6%;
[0074] (2) Preparation of reactant B: 170 g of trimethylene carbonate (TMC) and 30 g of glycolide (GA) were placed in a 3 L stainless steel reactor, and 0.01 wt % of stannous octoate catalyst and 0.13 wt % of dodecanol were added. The system temperature was raised to 170° C. under nitrogen protection, and polymerization reaction was carried out for 6 hours to obtain reactant B, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 1.68 dl / g. The tensile strength of reactant B obtained by mechanical test at 25° C. was 5 MPa, and the elongation at break was 409%;
[0075] (3) Preparation of PGLT5: 70 g of reactant A, 130 g of reactant B and 800 g of glycolide were added to a 3 L stainless steel reactor. Under nitrogen protection, the temperature was raised to 205°C and maintained for 4 hours to obtain PGLT5, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.86 dl / g.
[0076] The composition ratio determination and performance characterization of PGLT5 are the same as those in Example 1, see Table 1.
[0077] Example 6
[0078] Preparation of glycolide, DL-lactide, trimethylene carbonate PGLT copolymer 6 (PGLT6):
[0079] (1) Preparation of reactant A: 180 g of DL-lactide (LA) and 20 g of glycolide (GA) were placed in a 3 L stainless steel reactor, and 0.02% by weight of stannous octoate catalyst and 0.16% by weight of octadecyl alcohol were added. The system temperature was raised to 160° C. under nitrogen protection, and polymerization reaction was carried out for 8 hours to obtain reactant A, whose intrinsic viscosity measured at 25° C. in 0.1 g / dl chloroform was 2.83 dl / g. The tensile strength of reactant A obtained by mechanical test at 25° C. was 51 MPa, and the elongation at break was 11%;
[0080] (2) Preparation of reactant B: same as in Example 3;
[0081] (3) Preparation of PGLT6: 120 g of reactant A, 180 g of reactant B and 700 g of glycolide were added to a 3 L stainless steel reactor. Under nitrogen protection, the temperature was raised to 220°C and maintained for 4 hours to obtain PGLT6, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.65 dl / g.
[0082] The composition ratio determination and performance characterization of PGLT6 are the same as those in Example 1, see Table 1.
[0083] Example 7
[0084] The preparation of glycolide, L-lactide, trimethylene carbonate PGLT copolymer 7 (PGLT7) comprises the following steps:
[0085] Reactant A of Example 1 and reactant B of Example 4 were added into a 3L stainless steel reactor at a mass percentage of A / B / C of 25:13:62. The reactor was heated to 220°C under nitrogen protection and maintained for 4 hours to obtain PGLT7, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.57 dl / g.
[0086] The composition ratio determination and performance characterization of PGLT7 are the same as those in Example 1, see Table 1.
[0087] Embodiment 8:
[0088] Reactant A of Example 1 and reactant B of Example 4 were added into a 3L stainless steel reactor at a mass percentage of A / B / C of 5:20:75. Under nitrogen protection, the temperature was raised to 222°C and maintained for 4 hours to obtain PGLT8, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.53 dl / g.
[0089] Comparative Example 1
[0090] Preparation of glycolide, L-lactide, trimethylene carbonate random copolymer 1 (PGLTW1), the preparation method comprising the following steps:
[0091] 720 g of glycolide, 120 g of L-lactide and 160 g of trimethylene carbonate were placed in a 3L stainless steel reactor, 0.02% of stannous octoate catalyst and 0.02% by weight of octadecyl alcohol were added, the system temperature was raised to 205°C under nitrogen protection, and the reaction was carried out for 5 hours to obtain a PGLTW1 random copolymer, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.76 dl / g.
[0092] Comparative Example 2
[0093] The preparation of glycolide, L-lactide, trimethylene carbonate random copolymer 2 (PGLTW2) comprises the following steps:
[0094] 800 g of glycolide, 60 g of L-lactide and 140 g of trimethylene carbonate were placed in a 3L stainless steel reactor, 0.02% of stannous octoate catalyst and 0.02% by weight of octadecyl alcohol were added, the system temperature was raised to 210°C under nitrogen protection, and the reaction was carried out for 4.5 hours to obtain a PGLTW2 random copolymer, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.68 dl / g.
[0095] Comparative Example 3
[0096] Synthesis of PGA:
[0097] 600 g of glycolide was placed in a 3L stainless steel reactor, 0.01% of stannous octoate catalyst and 0.01% by weight of dodecanol were added, the system temperature was raised to 220°C under nitrogen protection, and the reaction was carried out for 2.5 hours to obtain a PGA homopolymer, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.69 dl / g.
[0098] Comparative Example 4
[0099] Synthesis of poly L-lactic acid (poly L-lactide PLLA):
[0100] The preparation method is the same as that of reactant A in Example 1.
[0101] Comparative Example 5
[0102] Synthesis of polydioxanone (PPDO):
[0103] 600 g of p-dioxanone monomer (PDO) was placed in a 3L stainless steel reactor, 0.02% of stannous octoate catalyst and 0.01% by weight of dodecanol were added, the system temperature was raised to 120°C under nitrogen protection, and the reaction was carried out for 24 hours to obtain a PPDOA homopolymer, whose intrinsic viscosity measured at 25°C in hexafluoroisopropanol with a concentration of 0.1 g / dl was 1.96 dl / g.
[0104] Comparative Example 6
[0105] Preparation of PGA and PPDO blends:
[0106] 420 g of PGA and 80 g of PPDO were physically blended and then injection molded into dumbbell-shaped test samples at an injection temperature of 228°C.
[0107] Comparative Example 7
[0108] Preparation of PGA and PPDO blends:
[0109] 400 g of PGA and 100 g of PPDO were physically blended and then injection molded into dumbbell sheet test samples at an injection temperature of 228°C.
[0110] Comparative Example 8
[0111] Preparation of PGA and PTMC blends:
[0112] 420 g of PGA and 80 g of PTMC were physically blended and then injection molded into dumbbell sheet test samples at an injection temperature of 228°C.
[0113] Detection and characterization:
[0114] 1. The products obtained in Examples 1-8 and Comparative Examples 1-8 were tested, and the results are shown in Table 1.
[0115] Table 1 Polymer performance results
[0116]
[0117]
[0118] As can be seen from Table 1, the absorbable copolymers PGLT prepared by Examples 1-8 of the present invention are compared with the random copolymers prepared in Comparative Example 1. Although the GA content in the polymers is similar, the absorbable copolymers prepared by the present invention have higher crystallinity and higher tensile yield strength, which can reach up to 76 MPa, which is much greater than the polydioxanone PPDO in Comparative Example 5. This result further confirms the conclusion that when the molecular composition of the materials is similar, the higher the crystallinity of the polymer, the higher the mechanical properties.
[0119] The melting peak of the absorbable copolymer PGLT prepared in Examples 1-7 of the present invention is 213-218°C, the melting peaks of the random copolymers of Comparative Examples 1 and 2 are lower than 213°C, and the melting peak of the PGA homopolymer of Comparative Example 3 is about 222°C. It can be seen that materials with low crystalline melting peak values are more flexible and easier to perform thermoplastic processing than materials with high crystalline melting peak values.
[0120] Compared with the low elongation at break and lack of toughness of the PGA homopolymer of Comparative Example 3 and the PLLA homopolymer of Comparative Example 4, the PGLT random copolymer and the PGLT copolymers prepared by the present invention 1-8 have higher elongation at break and better toughness.
[0121] The toughness and degradation time of PPDO in Comparative Example 5 are moderate, but the mechanical strength is low (tensile yield strength <30 MPa). Comparative Examples 6, 7 and 8 are all blends of PGA and soft materials, and the tensile strength and toughness can meet the application requirements.
[0122] It can be seen from Examples 1-8 that the mechanical strength and degradation time of the copolymers are different due to the different ratios of reactants A, reactant B and reactant C. The higher the content of LA (reactant A) and GA (reactant C) polymer segments in the hard segment, the higher the mechanical strength, and the contribution of the GA polymer segment to the mechanical strength is greater than that of the LA segment. Therefore, it can be seen that the polymer formed by replacing GA with LLA, or the polymer formed when the LLA content is greater than GA, although it still contains TMC polymer segments, the formed PGLT copolymer is very easy to relax under stress and produce permanent deformation.
[0123] 2. In vitro degradation mechanical properties test of the polymers obtained in Examples 1-8 and Comparative Examples 1-8
[0124] Test method: The test was carried out in a phosphate buffer solution at 37°C. The sample shape was a dumbbell sheet. The test method was consistent with that in Example 1. Samples were taken out for testing at different time points. The results are shown in Chart 2.
[0125] Table 2 In vitro degradation mechanical results of polymers
[0126]
[0127]
[0128] As shown in Table 2, the tensile strength maintenance time of the PGLT copolymers of Examples 1-8 obtained by the preparation method of the present invention is significantly higher than that of the PGLT random copolymers formed in Comparative Examples 1 and 2. This is mainly because the disordered arrangement of the monomers in the random copolymer reduces the crystallization of the PGA segment and increases the amorphous component that degrades faster. Although the degradation time of PGA in Comparative Example 3 and PLLA in Comparative Example 4 is higher than that of the random copolymer, the disadvantage is that the material lacks toughness. The PPDO in Comparative Example 5 has sufficient degradation strength maintenance time, but the strength and hardness are insufficient to prepare absorbable closure clips. The material strength maintenance of Comparative Examples 6 and 7 does not exceed 10 days. Comparative Example 8 is a composite material blended with PGA and PTMC. Although the degradation rate of PTMC therein is much slower than that of PGA, the degradation strength maintenance time is not significantly improved compared with PGA.
[0129] 3. The materials of Examples 1-8 and Comparative Examples 1-8 and polyoxymethylene were sequentially injection molded into absorbable tissue closure clips and then the performance was tested: closure force and degradation maintenance time. The results are shown in Table 3. Closure clip structure Figure 3 As shown. The temperature of the injection molding machine head and nozzle is 190℃-230℃, the injection pressure is 70-150MPa, and the injection speed is greater than 100mm / second. In the field of medical devices, the clamping force of the absorbable closing clip should be greater than 5N.
[0130] Test method for clamping force: Take two non-woven fabrics with a width of 5mm±1mm, overlap them in the center at the position where the closing clamp is clamped, fix the two non-woven fabrics on a mechanical testing machine, and then stretch the non-woven fabrics at a speed of 10mm / min until the closing clamp is pulled off or broken, and record the tension value at this time.
[0131] Table 3 Closing force results of closing clamp
[0132]
[0133] As can be seen from Table 3, the closure force degradation maintenance time of the absorbable closure clip prepared by using the PGLT copolymer prepared by Examples 1-8 of the present invention can be maintained for at least 14 days; compared with the closure clips supported by the random copolymers of Comparative Examples 1 and 2, the in vitro degradation time of the random copolymer closure clip does not exceed 10 days, which is much lower than that of the material prepared by the present invention; the PGA composite materials prepared by blending in Comparative Examples 6, 7 and 8 have a degradation time of less than 10 days; the closure force of the closure clip prepared by the PPDO material in Comparative Example 5 can only reach 15-16N in the initial stage. The low clamping force is prone to slippage and displacement during use, and cannot penetrate the fascia tissue; the PGA in Comparative Example 3 and the PLLA material in Comparative Example 4 are hard materials, and the prepared closure clips cannot be buckled and are prone to breakage when closed.
[0134] In summary, the PGLT copolymer prepared by the present invention has high strength and good toughness, and the degradation time can reach 14 days or more. Considering the mechanical properties and degradation time of the material, the PGLT copolymer is suitable for preparing absorbable tissue closure clips, soft tissue nails, suture clips, suture anchors, surgical sutures, puncture occluders or anal fistula occluders, etc.
Claims
1. A method for preparing an absorbable copolymer, characterized in that: The PGLT copolymer is formed by step-by-step copolymerization of glycolide, lactide and trimethylene carbonate. The weight percentage of glycolide in the PGLT copolymer is 60%-85%, the weight percentage of lactide is 5%-25%, and the weight percentage of trimethylene carbonate is 8%-25%. In the step-by-step copolymerization process, lactide and trimethylene carbonate are first polymerized to form a prepolymer and then copolymerized with glycolide. The PGLT copolymer contains three chain segments of polymerized glycolide, polymerized lactide and polymerized trimethylene carbonate. The steps are as follows: (1) Reactant A: lactide or lactide and glycolide are polymerized in the presence of an initiator and a catalyst to form a homopolymer or a copolymer; (2) Reactant B: trimethylene carbonate or trimethylene carbonate and glycolide are polymerized in the presence of an initiator and a catalyst to form a homopolymer or a copolymer; (3) Copolymerization: glycolide is used as reactant C. Reactant C is melt-blended with reactants B and A and polymerized in an air-isolated reactor to form a PGLT copolymer.
2. The method for preparing the absorbable copolymer according to claim 1, characterized in that: The preparation method comprises: (1) Reactant A: Add 0.01%-0.2% by weight of initiator and 0.01%-0.1% by weight of catalyst, add lactide and glycolide into the reactor respectively under nitrogen protection or vacuum conditions, raise the temperature to 150°C-180°C, maintain the reaction temperature for 6-15 hours, and perform ring-opening polymerization to obtain reactant A; (2) Reactant B: add 0.01%-0.2% by weight of initiator and 0.01%-0.1% by weight of catalyst, add trimethylene carbonate and glycolide into the reactor respectively under nitrogen protection or vacuum conditions, raise the temperature to 150°C-180°C, maintain the reaction temperature for 2-8 hours, and perform ring-opening polymerization to obtain reactant B; (3) Copolymerization: With glycolide as reactant C, reactant C is melt-blended with reactants A and B, and polymerized at 200°C-230°C in an air-isolated reactor to form a PGLT copolymer containing glycolide, lactide and trimethylene carbonate.
3. The method for preparing the absorbable copolymer according to claim 1 or 2, characterized in that: The initiator is a monohydric alcohol, a dihydric alcohol or a polyhydric alcohol among fatty alcohols, and the catalyst is stannous octoate.
4. The method for preparing the absorbable copolymer according to claim 1 or 2, characterized in that: The lactide is one or more of L-lactide, DL-lactide or D-lactide.
5. The method for preparing the absorbable copolymer according to claim 1 or 2, characterized in that: In reactant A, the weight percentage of glycolide is 0-20%, and in reactant B, the weight percentage of glycolide is 0-20%.
6. The absorbable copolymer obtained according to any one of the preparation methods of claims 1 to 5, characterized in that: The elastic modulus of the PGLT copolymer is 600MPa-2300MPa, the tensile yield strength is greater than 40MPa, and the tensile elongation at break is not less than 40%.
7. The absorbable copolymer according to claim 6, characterized in that: The elastic modulus of the PGLT copolymer is 800MPa-2000MPa, the tensile yield strength is greater than 50MPa, and the tensile elongation at break is not less than 50%.
8. The absorbable copolymer obtained by the preparation method according to any one of claims 1 to 5, characterized in that: The intrinsic viscosity of the PGLT copolymer measured in hexafluoroisopropanol at a concentration of 0.1 g / dl at 25° C. is 0.8-2.5 dl / g.
9. The absorbable copolymer obtained by the preparation method according to any one of claims 1 to 5, characterized in that: The PGLT copolymer has a tensile strength of not less than 5 MPa after being immersed in a phosphate buffer solution at 37° C. for 14 days.
10. An application of an absorbable copolymer, characterized in that: The absorbable copolymer can be used to prepare a tissue closure clip, a suture clip, a suture anchor, an anastomotic staple, a surgical suture, a puncture plugger or an anal fistula plugger.
Citation Information
Patent Citations
Plastic ligating clips
US4424810A
Multi-block biodegradable shape memory polymeric compound with regular structure and preparation thereof
CN101475677A
Medical biopolymer material with linear degradation as well as preparation and application of medical biopolymer material
CN117487140A
Absorbable segmented copolymer, preparation method, application and absorbable binding belt
CN117866183A
Triblock terpolymer, its use in medical products and process for its production
US6031069A