Binary polyether ester type defoaming agent and preparation method thereof
The waste leachate treatment is solved by using binary polyetherester defoaming agent prepared by esterification of long-carbon chain fatty alcohols, propylene oxide, ethylene oxide and dicarboxylic acid, carboxylic anhydride or carboxylic acid ester. The problem of poor bubble effect achieves efficient and environmentally friendly defoaming and foam suppression performance, avoiding the environmental harm of traditional defoaming agents.
Patent Information
- Application Number
- CN202411095160.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
AI Technical Summary
The existing defoaming agents have poor defoaming effect in the treatment of garbage leachate, and the polyether-modified silicone defoaming agents have poor foam inhibition ability. The polyether-modified silicone defoaming agents are prone to block the permeable membrane, and some components are harmful to the environment.
Long-carbon chain fatty alcohol, propylene oxide, ethylene oxide and dicarboxylic acid, carboxylic anhydride or carboxylic acid esters are used as raw materials, and esterified by block polyether compounds with dicarboxylic acid, carboxylic anhydride or carboxylic acid esters The binary polyetherester type defoaming agent was prepared by reaction, which had excellent defoaming and foam suppression properties.
It achieves better defoaming and foaming effects in the treatment of garbage leachate. It has a simple process, low cost, green and environmentally friendly, and avoids the environmental harm of traditional defoaming agents.
Smart Images

Figure CN118978684A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a defoamer and a preparation method thereof, in particular to a binary polyether ester defoamer and a preparation method thereof, and belongs to the field of environmental engineering additives. Background Art
[0002] Landfill leachate contains a large amount of heavy metal ions and difficult-to-biodegrade organic matter. It is a toxic and harmful high-concentration organic wastewater with complex pollutant composition, large fluctuations in water quality, high concentration of organic pollutants, high concentration of ammonia nitrogen, deep chroma, strong odor, high concentration of heavy metal ions and salt content, and strong toxicity. A large amount of foam is easily generated during the leachate treatment process, and it is difficult to control and eliminate it with ordinary defoamers. It is urgent to research and develop environmentally friendly defoamers with better defoaming effects for leachate treatment systems. At present, the defoamers used in leachate on the market are mainly silicones, polyethers, polyether-modified polysiloxanes, etc. Polyether defoamers have poor foam suppression ability, resulting in increased addition and increased costs; polyether-modified silicon defoamers have good instantaneous defoaming performance and good high temperature resistance, but are easy to clog the permeation membrane system.
[0003] Invention patent CN102126763A discloses a defoamer suitable for landfill leachate, which is composed of nonylphenol polyoxyethylene ether, alkylphenol polyoxyethylene ether, glycerol polyoxypropylene polyoxyethylene ether, low-carbon alcohol and flocculant. However, nonylphenol polyoxyethylene ether is harmful to the environment and toxic to aquatic organic systems, and has been gradually banned. The defoamer disclosed in invention patent CN105504290A is an emulsion-type landfill leachate defoamer prepared with white carbon black and polyether-modified polysiloxane as the main active substances, and an emulsifier and a thickener are added. It has good defoaming and anti-foaming capabilities, but the defoamer with white carbon black and polyether-modified polysiloxane as the main active substances used in the leachate will cause the osmotic membrane to be blocked, thereby making the leachate treatment difficult and increasing the cost.
[0004] Polyether ester defoamer is a high-efficiency defoamer developed on the basis of polyether defoamers. It has the characteristics of high temperature resistance, low surface tension and good stability of polyether defoamers. Since the terminal hydroxyl groups are esterified, the esterified polyether ester has enhanced lipophilicity, smaller surface tension and stronger defoaming ability. Existing polyether ester defoamers usually use glycerol / 12-18 alcohol as initiators to prepare glycerol / fatty alcohol polyoxyethylene polyoxypropylene ether, which is then esterified with lauric acid or oleic acid to obtain polyether ester defoamer.
[0005] Invention patent CN202311046111.1 discloses a method for preparing a high-carbon alcohol polyether ester defoamer. It includes the following steps: (1) using a fatty alcohol with a carbon chain length of 12 or more as an initiator, adding ethylene oxide and propylene oxide for polymerization, and obtaining a high-carbon fatty alcohol polyoxypropylene polyoxyethylene ether; (2) reacting the high-carbon fatty alcohol polyoxypropylene polyoxyethylene ether with a fatty acid under the action of a catalyst to obtain a high-carbon alcohol polyether ester for a defoamer. The preparation method of the high-carbon alcohol polyether ester provided by the present invention has the advantages of simple production process, low cost, excellent product defoaming performance and anti-foaming performance, good storage stability, etc., but the polyether ester is a monocarboxylic acid ester, and only one polyether segment is introduced. Invention patent CN201710379731.5 discloses a novel polyether ester defoamer and a preparation method thereof. Using higher fatty alcohol as the initiator, reacting with ethylene oxide and propylene oxide, fatty alcohol polyoxyethylene polyoxypropylene ether is prepared; fatty alcohol polyoxyethylene polyoxypropylene ether is esterified with fatty acid to prepare polyether ester. The defoaming performance of polyether ester defoamers is closely related to the type and carbon chain length of fatty acid. The fatty acids introduced in the polyether ester defoamers reported are all single-chain fatty acids, and no dibasic polyether ester defoamers of dibasic carboxylic acids, dibasic carboxylic acid anhydrides or dibasic carboxylic acid esters have been found.
[0006] The present invention provides a binary polyether ester defoamer and a preparation method thereof. Long-chain fatty alcohol, propylene oxide, ethylene oxide, dicarboxylic acid, dicarboxylic acid anhydride or dicarboxylic acid ester are used as raw materials. The preparation process comprises the following steps: preparing a block polyether compound from a long-chain fatty alcohol, propylene oxide or ethylene oxide; preparing a binary polyether ester defoamer from a block polyether compound and dicarboxylic acid, dicarboxylic acid anhydride or dicarboxylic acid ester. The binary polyether ester defoamer of the present invention is suitable for the defoaming and defoaming process of landfill leachate, and has excellent defoaming and defoaming performance; and has the advantages of simple preparation process, green environmental protection, and convenient application. Summary of the invention
[0007] Purpose of the invention: The first purpose of the present invention is to provide a binary polyether ester type defoamer used for defoaming treatment of landfill leachate; the second purpose of the present invention is to provide a method for preparing a binary polyether ester type defoamer used for defoaming treatment of landfill leachate.
[0008] Technical solution: In order to achieve the above-mentioned invention object, the present invention provides the following technical solution:
[0009] A binary polyether ester defoamer and a preparation method thereof, comprising the following steps:
[0010] (1) Block polyether compounds
[0011] A long-chain fatty alcohol (with carbon number ≥ 12) is used as an initiator, a catalyst is added, and propylene oxide and ethylene oxide are added in sequence to carry out polymerization reaction to obtain a segmented fatty alcohol polyoxypropylene polyoxyethylene ether;
[0012] (2) Polyether ester
[0013] Block type fatty alcohol polyoxypropylene polyoxyethylene ether, adding catalyst and fatty acid, esterification reaction, to obtain fatty alcohol polyoxypropylene polyoxyethylene ether fatty acid ester;
[0014] The general structural formula of the binary polyether ester defoamer is:
[0015]
[0016] Wherein, R represents fatty alcohol units of different chain lengths; P represents propylene oxide units; E represents ethylene oxide units; and A represents dicarboxylic acid, dicarboxylic acid anhydride or dicarboxylic acid ester units.
[0017] Furthermore, in step (1), the fatty alcohol is lauryl alcohol, tetradecanol, hexadecanol, octadecanol, eicosanol, C12-14 mixed alcohol, C14-16 mixed alcohol, C16-18 mixed alcohol or C18-20 mixed alcohol; in step (1), the mass ratio of propylene oxide to ethylene oxide is (30-60):(40-70); in step (1), the catalyst is sodium hydroxide or potassium hydroxide; and in step (1), the amount of the catalyst added is 1.0%-1.5% of the mass of the fatty alcohol.
[0018] Furthermore, in step (1), the polymerization reaction is carried out under a pressure of 0.03 to 0.3 MPa, at a temperature of 120 to 150° C., and for a time of 180 to 360 min.
[0019] Furthermore, in step (1), the number average molecular weight of the block fatty alcohol polyoxypropylene polyoxyethylene ether is 2000-4000.
[0020] Further, in step (2), the dicarboxylic acid, dicarboxylic acid anhydride or dicarboxylic acid ester is malonic acid, succinic acid, glutaric acid, adipic acid, 1,4-cyclohexanedicarboxylic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, tridecanedicarboxylic acid, tetradecanedicarboxylic acid, pentadecanedicarboxylic acid, hexadecanedicarboxylic acid, heptadecanedicarboxylic acid, octadecanedicarboxylic acid, nonadecanedicarboxylic acid, eicosanedicarboxylic acid, heneicosanedicarboxylic acid, docosanedicarboxylic acid, tricosanedicarboxylic acid, tetracosanedicarboxylic acid, pentacosanedicarboxylic acid, hexacosanedicarboxylic acid, succinic anhydride, maleic anhydride, glutaric anhydride, 3-methyl-glutaric anhydride, 2,2-dimethyl-glutaric anhydride, 3,3-dimethyl-glutaric anhydride, cis-1,2-cyclohexanedicarboxylic acid anhydride, adipic acid anhydride, dimethyl malonate, diethyl malonate, dibutyl malonate, dimethyl glutarate, diethyl glutarate, dibutyl glutarate, dimethyl suberate, diethyl suberate, dibutyl suberate, dimethyl azelaate, diethyl azelaate, dibutyl azelaate, dimethyl sebacate, diethyl sebacate, dibutyl sebacate; the esterification reaction temperature in step (2) is 120-140° C., and the reaction time is 120-300 min; the molar ratio of the block type fatty alcohol polyoxypropylene polyoxyethylene ether to the fatty acid in step (2) is 1.5-2.2; the catalyst in step (2) is one of toluenesulfonic acid, sulfuric acid, phosphoric acid, and hypophosphorous acid; the amount of the catalyst added in step (2) is 0.2-0.8% of the total mass of the block type fatty alcohol polyoxypropylene polyoxyethylene ether and the fatty acid.
[0021] The present invention provides a binary polyether ester defoamer and a preparation method thereof. Long-chain fatty alcohol, propylene oxide, ethylene oxide, dicarboxylic acid, dicarboxylic acid anhydride or dicarboxylic acid ester are used as raw materials. The preparation process comprises the following steps: preparing a block polyether compound from a long-chain fatty alcohol, propylene oxide or ethylene oxide; preparing a binary polyether ester defoamer from a block polyether compound and dicarboxylic acid, dicarboxylic acid anhydride or dicarboxylic acid ester. The binary polyether ester defoamer of the present invention is suitable for the defoaming and defoaming process of landfill leachate, and has excellent defoaming and defoaming performance; and has the advantages of simple preparation process, green environmental protection, and convenient application.
[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0023] (1) Block-type fatty alcohol polyoxypropylene polyoxyethylene ether has lower surface tension than traditional fatty alcohol polyoxyethylene polyoxypropylene ether;
[0024] (2) The introduction of dicarboxylic acid, dicarboxylic anhydride or dicarboxylic ester into dibasic polyether ester defoamers has better defoaming ability, excellent degassing and anti-foaming effects than traditional polyether ester defoamers;
[0025] (3) Binary polyether ester defoaming agent has the advantages of simple process, low cost, green environmental protection and easy application. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The general structure of binary polyether ester defoamer DETAILED DESCRIPTION
[0027] The technical solution of the present invention is further described below in conjunction with embodiments.
[0028] Example 1
[0029] (1) Block polyether compounds
[0030] In the reactor, nitrogen is introduced, 250 g of dodecanol and 3 g of potassium hydroxide are added, the temperature is raised to 120° C., mixed evenly, 40 g of propylene oxide is introduced, the pressure in the reactor is controlled at 0.3 MPa, the temperature is raised to 130° C., stirred for 60 min, 50 g of ethylene oxide is continued to be added, the temperature is raised to 140° C., the reaction is carried out for 30 min, vacuum degassing is performed, the temperature is cooled to room temperature and the material is discharged to obtain a crude product of block fatty alcohol polyoxypropylene polyoxyethylene ether; the crude product of block fatty alcohol polyoxypropylene polyoxyethylene ether is adjusted to pH value with aqueous phosphoric acid solution, dehydrated with sodium silicate, and filtered to obtain a refined block fatty alcohol polyoxypropylene polyoxyethylene ether product; the GPC test molecular weight is 3200 g / mol.
[0031] (2) Binary polyether ester compounds
[0032] Into the reactor, nitrogen was introduced, 180 g of refined segmented fatty alcohol polyoxypropylene polyoxyethylene ether, 40 g of glutaric acid, and 0.5 g of p-toluenesulfonic acid as a catalyst were added, the temperature was raised to 140°C, the acid value of the reaction system was tested every 60 minutes, the reaction was stopped until the acid value no longer changed, the temperature was lowered to 70°C, triethanolamine was added, the pH value was adjusted to neutral, a saturated sodium chloride solution was added for washing, and the reaction was dried to obtain segmented fatty alcohol polyoxypropylene polyoxyethylene ether ester, i.e., binary polyether ester defoamer 01.
[0033] Example 2
[0034] (1) Block polyether compounds
[0035] In the reactor, nitrogen is introduced, 250 g of dodecanol and 3 g of potassium hydroxide are added, the temperature is raised to 120° C., mixed evenly, 40 g of propylene oxide is introduced, the pressure in the reactor is controlled at 0.3 MPa, the temperature is raised to 130° C., stirred for 60 min, 50 g of ethylene oxide is continued to be added, the temperature is raised to 140° C., the reaction is carried out for 30 min, vacuum degassing is performed, the temperature is cooled to room temperature and the material is discharged to obtain a crude product of block fatty alcohol polyoxypropylene polyoxyethylene ether; the crude product of block fatty alcohol polyoxypropylene polyoxyethylene ether is adjusted to pH value with aqueous phosphoric acid solution, dehydrated with sodium silicate, and filtered to obtain a refined block fatty alcohol polyoxypropylene polyoxyethylene ether product; the GPC test molecular weight is 3200 g / mol.
[0036] (2) Binary polyether ester compounds
[0037] Into the reactor, nitrogen was introduced, 180 g of refined segmented fatty alcohol polyoxypropylene polyoxyethylene ether, 46 g of maleic anhydride, and 0.5 g of p-toluenesulfonic acid as a catalyst were added, the temperature was raised to 140°C, the acid value of the reaction system was tested every 60 minutes, the reaction was stopped until the acid value no longer changed, the temperature was lowered to 70°C, triethanolamine was added, the pH value was adjusted to neutral, a saturated sodium chloride solution was added for washing, and the reactor was dried to obtain segmented fatty alcohol polyoxypropylene polyoxyethylene ether ester, i.e., binary polyether ester defoamer 02.
[0038] Example 3
[0039] (1) Block polyether compounds
[0040] In the reactor, nitrogen is introduced, 300 g of octadecyl alcohol and 4 g of potassium hydroxide are added, the temperature is raised to 120° C., mixed evenly, 50 g of propylene oxide is introduced, the pressure in the reactor is controlled to 0.3 MPa, the temperature is raised to 130° C., stirred for 60 min, 50 g of ethylene oxide is continued to be added, the temperature is raised to 140° C., the reaction is carried out for 30 min, vacuum degassing is carried out, the temperature is cooled to room temperature and the material is discharged to obtain a crude product of block fatty alcohol polyoxypropylene polyoxyethylene ether; the crude product of block fatty alcohol polyoxypropylene polyoxyethylene ether is adjusted to pH value with aqueous phosphoric acid solution, dehydrated with sodium silicate, and filtered to obtain a refined block fatty alcohol polyoxypropylene polyoxyethylene ether product; the GPC test molecular weight is 3400 g / mol.
[0041] (2) Binary polyether ester compounds
[0042] Into the reactor, nitrogen was introduced, 180 g of refined segmented fatty alcohol polyoxypropylene polyoxyethylene ether, 40 g of adipic acid, and 0.5 g of p-toluenesulfonic acid as a catalyst were added, the temperature was raised to 140°C, the acid value of the reaction system was tested every 60 minutes, the reaction was stopped until the acid value no longer changed, the temperature was lowered to 70°C, triethanolamine was added, the pH value was adjusted to neutral, a saturated sodium chloride solution was added for washing, and the reaction was dried to obtain segmented fatty alcohol polyoxypropylene polyoxyethylene ether ester, i.e., binary polyether ester type defoamer 03.
[0043] Example 4
[0044] (1) Block polyether compounds
[0045] In a reactor, nitrogen is introduced, 300 g of hexadecanol and 4 g of potassium hydroxide are added, the temperature is raised to 120° C., mixed evenly, 60 g of propylene oxide is introduced, the pressure in the reactor is controlled at 0.4 MPa, the temperature is raised to 130° C., stirred for 60 min, 50 g of ethylene oxide is continued to be added, the temperature is raised to 140° C., reacted for 30 min, vacuumed and degassed, cooled to room temperature and discharged to obtain a crude product of segmented fatty alcohol polyoxypropylene polyoxyethylene ether; the crude product of segmented fatty alcohol polyoxypropylene polyoxyethylene ether is adjusted to pH value with aqueous phosphoric acid solution, dehydrated with sodium silicate, and filtered to obtain a refined segmented fatty alcohol polyoxypropylene polyoxyethylene ether product; the GPC test molecular weight is 3300 g / mol.
[0046] (2) Binary polyether ester compounds
[0047] Into the reactor, nitrogen was introduced, 180 g of refined segmented fatty alcohol polyoxypropylene polyoxyethylene ether, 40 g of cis-1,2-cyclohexanedicarboxylic anhydride, and 0.5 g of p-toluenesulfonic acid as a catalyst were added, the temperature was raised to 140°C, the acid value of the reaction system was tested every 60 minutes, the reaction was stopped until the acid value no longer changed, the temperature was lowered to 70°C, triethanolamine was added, the pH value was adjusted to neutral, a saturated sodium chloride solution was added for washing, and the reactor was dried to obtain segmented fatty alcohol polyoxypropylene polyoxyethylene ether ester, i.e., binary polyether ester defoamer 04.
[0048] Example 5
[0049] (1) Block polyether compounds
[0050] In the reactor, nitrogen is introduced, 300 g of octadecyl alcohol and 4 g of potassium hydroxide are added, the temperature is raised to 120° C., mixed evenly, 50 g of propylene oxide is introduced, the pressure in the reactor is controlled at 0.3 MPa, the temperature is raised to 130° C., stirred for 60 min, 50 g of ethylene oxide is continued to be added, the temperature is raised to 140° C., the reaction is carried out for 30 min, vacuum degassing is performed, the temperature is cooled to room temperature and the material is discharged to obtain a crude product of block fatty alcohol polyoxypropylene polyoxyethylene ether; the crude product of block fatty alcohol polyoxypropylene polyoxyethylene ether is adjusted to pH value with aqueous phosphoric acid solution, dehydrated with sodium silicate, and filtered to obtain a refined block fatty alcohol polyoxypropylene polyoxyethylene ether product; the GPC test molecular weight is 3400 g / mol.
[0051] (2) Binary polyether ester compounds
[0052] Into the reactor, nitrogen was introduced, 200 g of refined segmented fatty alcohol polyoxypropylene polyoxyethylene ether, 40 g of azelaic acid, and 0.5 g of p-toluenesulfonic acid as a catalyst were added, the temperature was raised to 140°C, the acid value of the reaction system was tested every 60 minutes, the reaction was stopped until the acid value no longer changed, the temperature was lowered to 70°C, triethanolamine was added, the pH value was adjusted to neutral, saturated sodium chloride solution was added for washing, and the reaction was dried to obtain segmented fatty alcohol polyoxypropylene polyoxyethylene ether ester, i.e., binary polyether ester type defoamer 05.
[0053] Example 6
[0054] (1) Block polyether compounds
[0055] In a reactor, nitrogen is introduced, 300 g of hexadecanol and 4 g of potassium hydroxide are added, the temperature is raised to 120° C., mixed evenly, 60 g of propylene oxide is introduced, the pressure in the reactor is controlled at 0.4 MPa, the temperature is raised to 130° C., stirred for 60 min, 50 g of ethylene oxide is continued to be added, the temperature is raised to 140° C., reacted for 30 min, vacuumed and degassed, cooled to room temperature and discharged to obtain a crude product of segmented fatty alcohol polyoxypropylene polyoxyethylene ether; the crude product of segmented fatty alcohol polyoxypropylene polyoxyethylene ether is adjusted to pH value with aqueous phosphoric acid solution, dehydrated with sodium silicate, and filtered to obtain a refined segmented fatty alcohol polyoxypropylene polyoxyethylene ether product; the GPC test molecular weight is 3300 g / mol.
[0056] (2) Binary polyether ester compounds
[0057] Into the reactor, nitrogen was introduced, 180 g of refined segmented fatty alcohol polyoxypropylene polyoxyethylene ether, 40 g of maleic anhydride, and 0.5 g of p-toluenesulfonic acid as a catalyst were added, the temperature was raised to 140°C, the acid value of the reaction system was tested every 60 minutes, the reaction was stopped until the acid value no longer changed, the temperature was lowered to 70°C, triethanolamine was added, the pH value was adjusted to neutral, a saturated sodium chloride solution was added for washing, and the reactor was dried to obtain segmented fatty alcohol polyoxypropylene polyoxyethylene ether ester, i.e., binary polyether ester defoamer 06.
[0058] Examples 1-6 of binary polyether ester defoamers prepared using different raw materials are summarized in Table 1. According to the National Standard of the People's Republic of China GB / T 21885-2008 (Textile printing and dyeing auxiliaries, defoamers, determination of defoaming effect), the defoaming performance of binary polyether ester defoamers was evaluated, and the results are shown in Table 1.
[0059] Table 1 Preparation of binary polyether ester defoamer and evaluation of defoaming performance
[0060]
Claims
1. A method for preparing a binary polyether ester defoamer, It is characterized in that The steps include: (1) Block fatty alcohol polyoxyethylene polyoxypropylene ether A long-chain fatty alcohol (with carbon number ≥ 12) is used as an initiator, a catalyst is added, and propylene oxide and ethylene oxide are added in sequence to carry out polymerization reaction to obtain a segmented fatty alcohol polyoxypropylene polyoxyethylene ether; (2) Polyether ester Block type fatty alcohol polyoxypropylene polyoxyethylene ether, adding catalyst and fatty acid, esterification reaction, to obtain fatty alcohol polyoxypropylene polyoxyethylene ether fatty acid ester; The general structural formula of the binary polyether ester defoamer is: Wherein, R represents fatty alcohol units of different chain lengths; P represents propylene oxide units; E represents ethylene oxide units; and A represents dicarboxylic acid, dicarboxylic acid anhydride or dicarboxylic acid ester units.
2. The method for preparing the binary polyether ester defoamer according to claim 1, Features: The fatty alcohol in the step (1) is dodecanol, tetradecanol, hexadecanol, octadecanol, eicosanol, C12-14 mixed alcohol, C14-16 mixed alcohol, C16-18 mixed alcohol or C18-20 mixed alcohol; the mass ratio of propylene oxide to ethylene oxide in the step (1) is (30-60):(40-70); the catalyst in the step (1) is sodium hydroxide or potassium hydroxide; the amount of the catalyst added in the step (1) is 1.0%-1.5% of the mass of the fatty alcohol.
3. The method for preparing the binary polyether ester defoamer according to claim 1, Features: The polymerization reaction in step (1) is carried out under a pressure of 0.03-0.3 MPa, a temperature of 120-150° C. and a time of 180-360 min.
4. The method for preparing the binary polyether ester defoamer according to claim 1, Features: The number average molecular weight of the block fatty alcohol polyoxypropylene polyoxyethylene ether in the step (1) is 2000-4000.
5. The method for preparing the binary polyether ester defoamer according to claim 1, Features: The dicarboxylic acid, dicarboxylic acid anhydride or dicarboxylic acid ester in the step (2) is malonic acid, succinic acid, glutaric acid, adipic acid, 1,4-cyclohexanedicarboxylic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, tridecanedicarboxylic acid, tetradecanedicarboxylic acid, pentadecanedicarboxylic acid, hexadecanedicarboxylic acid, heptadecanedicarboxylic acid, octadecanedicarboxylic acid, nonadecanedicarboxylic acid, eicosanedicarboxylic acid, heneicosanedicarboxylic acid, docosanedicarboxylic acid, tricosanedicarboxylic acid, tetracosanedicarboxylic acid, pentacosanedicarboxylic acid, hexacosanedicarboxylic acid, succinic anhydride, maleic anhydride, glutaric anhydride, 3-methyl-glutaric anhydride, 2,2-dimethyl-glutaric anhydride, 3,3-dimethyl-glutaric anhydride, cis-1,2-cyclohexanedicarboxylic anhydride, adipic anhydride, malonic acid dicarboxylic acid, The invention relates to a method for preparing the present invention wherein the present invention comprises the following steps: the step of preparing the present invention comprises: a) preparing a methyl ester, diethyl malonate, dibutyl malonate, dimethyl glutarate, diethyl glutarate, dibutyl glutarate, dimethyl suberate, diethyl suberate, dibutyl suberate, dimethyl azelaate, diethyl azelaate, dibutyl azelaate, dimethyl sebacate, diethyl sebacate, and dibutyl sebacate; the esterification reaction temperature in the step (2) is 120-140° C., and the reaction time is 120-300 min; the molar ratio of the block type fatty alcohol polyoxypropylene polyoxyethylene ether to the fatty acid in the step (2) is 1.5-2.2; the catalyst in the step (2) is one of p-toluenesulfonic acid, sulfuric acid, phosphoric acid, and hypophosphorous acid; the amount of the catalyst added in the step (2) is 0.2-0.8% of the total mass of the block type fatty alcohol polyoxypropylene polyoxyethylene ether and the fatty acid.