Method for preparing simple reversible thermochromic spherical cholesteric liquid crystal film

Through homogeneous solution phase separation technology and gradient spin coating and drying process, the problems of complex and poor stability of traditional liquid crystal reversible temperature variable materials are solved, and the uniform dispersion and efficient color distortion of spherical cholesteric liquid crystals are achieved. Color-changing labels and smart materials.

CN118978728AActive Publication Date: 2024-11-19GUANGDONG UNIV OF TECH +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411348029.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-19
Estimated Expiration
2044-09-26

AI Technical Summary

Technical Problem

The preparation process of traditional liquid crystal reversible temperature variable materials is complex, the emulsion method and liquid crystal capsule method have problems such as complex operation, poor stability, and uneven color display, and the range of commonly used polymers is limited.

Method used

Using homogeneous solution phase separation technology, the homogeneous liquid crystal and chiral agent are mixed with polylactic acid to form a transparent homogeneous solution, and the uniform dispersion of liquid crystals and spherical gallbladder are achieved through gradient spin coating and gradual drying. The formation of steroidal liquid crystals.

Benefits of technology

The uniform particle size distribution and reversible color discoloration effect of spherical cholesteric liquid crystals are achieved, the stability and response sensitivity of the material are improved, the preparation process is simplified, and the influence of surfactants and shear forces is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978728A_ABST
    Figure CN118978728A_ABST
Patent Text Reader

Abstract

The invention relates to the field of reversible variable-temperature ink, and discloses a method for preparing a simple and reversible thermochromic spherical cholesteric liquid crystal film, which comprises the following steps: taking nematic liquid crystal and chiral agent liquid crystal as a liquid crystal mixture, and dissolving polylactic acid and the liquid crystal mixture through a benign solution of the polylactic acid and the liquid crystal mixture to form a homogeneous solution; at the temperature of 10-40 DEG C, the homogeneous solution in the step S1 is spin-coated on a substrate in the mode that the spin-coating rotating speed is gradually increased from 50-100 rpm to 7000-8000 rpm in a gradient mode; and after spin-coating is completed, drying by adopting a gradual heating mode, and naturally cooling to obtain the reversible thermochromic film. According to the invention, a homogeneous solution phase separation technology is adopted, and a matched process is adopted, so that the phase separation cholesteric liquid crystal not only can change color, but also can avoid the failure of liquid crystal packaging, and can avoid the influence of a surfactant, a shearing force and a core-wall ratio. The reversible thermochromic film has the characteristics of high color change sensitivity, fast response and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of reversible temperature-variable ink, and in particular to a method for simply preparing a spherical cholesteric liquid crystal color-changing film that is reversibly temperature-sensitive and color-changing. Background Art

[0002] There are currently two common methods for preparing liquid crystal reversible temperature-changing materials:

[0003] Emulsion method. Through shear force, a structure similar to "O / W" is formed between the liquid crystal and the hydrophilic polymer, that is, the structure of the water phase enveloping the oil phase. At this time, the system is a coexistence of two phases, which is a metastable structure in thermodynamics. At this time, the liquid crystal exists in the polymer in the form of droplets. If necessary, a surfactant needs to be added to maintain the normal shape of the droplets. Commonly used polymers include polyvinyl alcohol. The surfactant has an effect on the orientation of the liquid crystal, which will affect the color change and the color change range. At the same time, the shear force action time needs to be strictly controlled: if the action time is too short, the droplets will be too large, the stability will be poor, and it will be easy to break the emulsion. If the action time is too long, the droplets will be too small, and the light scattering effect will be stronger. Secondly, there are fewer hydrophilic polymer systems, and it is impossible to effectively broaden the range of available polymers.

[0004] Liquid crystal capsule method. First, the cholesteric liquid crystal needs to be oriented in an aqueous solution of a specific polymer, and then the liquid crystal droplets dispersed in the polymer are polymerized to form a capsule wall by emulsion polymerization, and then washed with water several times to remove other polymer impurities. Then blended with the polymer matrix, the liquid crystal capsules are evenly dispersed through shear force. This method is complicated to operate and the process is cumbersome. Corresponding disadvantages: during polymerization, the amount of liquid crystal and polymer wall needs to correspond one to one, otherwise the core-wall ratio will be too high or too low, which will affect the scattering of light and thus affect the color display; the blending of the polymer matrix will change the viscosity of the system, making the dispersion of the liquid crystal capsules uneven, thereby affecting the color display. Summary of the invention

[0005] In order to solve the problems of complex preparation process of traditional thermochromic films, the present invention proposes a method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film. Through the homogeneous solution phase separation technology, the liquid crystal is evenly dispersed in the polymer, and spherical cholesteric liquid crystals with uniform particle size can be formed in the polymer, which can respond and reversibly change color within a certain temperature range.

[0006] To achieve the above object, the present invention provides a method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film, which comprises the following steps:

[0007] S1, using nematic liquid crystal and chiral liquid crystal as a liquid crystal mixture, dissolving the polylactic acid and liquid crystal mixture by a benign solution of the two to form a transparent homogeneous solution;

[0008] S2, spin coating the homogeneous solution of step S1 on the substrate in a manner of increasing the spin coating speed from 50-200 rpm to 7000-8000 rpm, wherein each spin coating gradient is maintained for 30-90 s, and the spin coating thickness of each spin coating gradient is 5-25 μm, wherein the substrate can be a glass or plastic sheet, and after coating, the liquid crystal mixture forms a spherical cholesteric liquid crystal with uniform particle size;

[0009] S3. After the spin coating is completed, the spin-coated homogeneous solution is dried by gradually increasing the temperature to completely evaporate the solvent. After natural cooling, a reversible thermochromic film is finally obtained.

[0010] As a further preferred technical solution of the present invention, in step S1, polylactic acid accounts for 70-99% of the total mass of the polylactic acid and liquid crystal mixture, and the liquid crystal mixture accounts for 1-30% of the total mass of the polylactic acid and liquid crystal mixture; the nematic liquid crystal accounts for 50-99% of the total mass of the liquid crystal mixture, and the chiral agent accounts for 1-50% of the total mass of the liquid crystal mixture.

[0011] As a further preferred technical solution of the present invention, in step S1, the benign solution is one or a mixture of two or more of methanol, ethanol, isopropanol, acetone, dimethyl sulfoxide, dichloromethane, chloroform, acetonitrile, tetrahydrofuran, ethyl acetate, n-hexane, toluene, xylene, n-butanol, acetic acid, and pyridine.

[0012] As a further preferred technical solution of the present invention, the nematic phase liquid crystal is at least one of 4-cyano-4'-nonyloxybiphenyl, 4-cyano-4'-hexyloxybiphenyl, 4-cyano-4'-heptyloxybiphenyl, 4-cyano-4'-octyloxybiphenyl, 4-(4-cyanophenoxy)-4'-octylbiphenyl, and 4-cyano-4'-dodecylbiphenyl; the chiral agent liquid crystal is at least one of R5011, S5011, R811, and S811.

[0013] As a further preferred technical solution of the present invention, in step S2, the spin coating speed increases from 50-100 rpm to 7000-8000 rpm and is divided into at least three gradients. Further preferably, the spin coating speed increases in five stages, specifically: the spin coating speed in the first stage is 50-200 rpm, and the holding time is 50-60 s; the spin coating speed in the second stage is 200-500 rpm, and the holding time is 50-60 s; the spin coating speed in the third stage is 500-1000 rpm, and the holding time is 50-60 s; the speed in the fourth stage is 1500-3000 rpm, and the holding time is 50-60 s; the fifth stage is 7000 rpm, and the holding time is 50-60 s.

[0014] As a further preferred technical solution of the present invention, in step S1, a homogeneous solution is formed by adding a stirrer for stirring at a speed of 500-1500 rpm for 1-6 hours; or shaking on a shaker for 2-3 hours; or cleaning with an ultrasonic cleaner at 40KHz for 5 seconds to one hour.

[0015] As a further preferred technical solution of the present invention, in step S3, drying can be carried out by one of ultraviolet drying, infrared drying, hot air heating drying, and hot stage heating drying.

[0016] As a further preferred technical solution of the present invention, in step S3, drying is performed at a heating rate of 5-10°C every 5 minutes from room temperature, and each 5-10°C heating is maintained for 1-5 minutes, and the maximum temperature does not exceed 200°C.

[0017] According to another aspect of the present invention, the present invention also provides a reversible thermochromic film prepared by the above method.

[0018] The present invention adopts homogeneous solution phase separation technology and a phase-matching process to achieve phase separation of cholesteric liquid crystals that not only change color but also form spherical cholesteric liquid crystals with uniform particle size, while avoiding liquid crystal encapsulation failure and the influence of surfactants, shear force, and core-to-wall ratio.

[0019] The invention adopts homogeneous solution phase separation technology to prepare a reversible, temperature-sensitive color-changing spherical cholesteric liquid crystal film, which has the characteristics of high color-changing sensitivity, fast response and good stability.

[0020] Compared with the traditional technology, the method of the present invention is simpler to operate and can efficiently prepare a reversible thermochromic spherical cholesteric liquid crystal material. The reversible thermochromic film can change color according to the change of temperature and can be applied to color-changing labels, anti-counterfeiting encryption, smart materials and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0022] Figure 1 Schematic diagram of the preparation of reversible thermochromic ink.

[0023] Figure 2 is the absorption wavelength of the color change temperature of the film sample prepared in Example 1.

[0024] Figure 3 These are observation pictures of the thin film sample under POM (polarizing microscope) during the drying and film-forming process of Example 1: the left picture was taken when the drying temperature was maintained at 80°C; the right picture was taken when the film was cooled to room temperature (20°C).

[0025] Figure 4 The film sample prepared in Example 1 was observed and counted under a POM (polarizing microscope) after three days (20°C).

[0026] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION

[0027] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0028] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0029] Example 1

[0030] like Figure 1 As shown, the method for preparing the reversibly thermochromic spherical cholesteric liquid crystal film proposed in this embodiment specifically comprises the following steps:

[0031] S1. Prepare a homogeneous solution of liquid crystal:

[0032] Polylactic acid was used as the polymer matrix, and R5011 and 8CB were used as the liquid crystal mixture; 47 mg of polylactic acid, 1.05 mg of R5011 and 1.95 mg of 8CB were dissolved in 1 ml of chloroform. The dissolution process was stirred on a stirrer (stirring speed was 1000 rpm, time was 6 h). In this process, multiple components were evenly dispersed in the solvent to form a homogeneous solution, which was a uniform transparent liquid.

[0033] S2, gradient spin coating

[0034] Dynamic spin coating was adopted, wherein: the first stage spin coating speed was 200 rpm, the time was 60 s, the second stage spin coating speed was 500 rpm, the time was 60 s, the third stage spin coating speed was 1000 rpm, the time was 60 s, the fourth stage speed was 3000 rpm, the time was 60 s, the fifth stage was 7000 rpm, the time was 60 s, the amount of each spin coating was 250 μL, the total coating thickness was 80 μm, and the transparent liquid was coated on the glass substrate. In this process, gradient spin coating was adopted, which provided favorable conditions for the stable separation of the polymer and liquid crystal mixture and the self-assembly of the liquid crystal polymer to form cholesteric liquid crystal.

[0035] S3, Drying and Film Forming

[0036] The hot-plate drying method was used, starting from 20°C and increasing the temperature by 10°C / 5 min to 100°C, where each temperature increase was 10°C and maintained for 5 min to dry the transparent liquid coated on the glass substrate, and then naturally cooled to finally obtain a reversible thermochromic film. The volatilization rate was regulated by gradient heating to achieve stable separation of the polymer and liquid crystal mixture phases, and the liquid crystal mixture was successfully self-assembled into cholesteric liquid crystal. Only when the cholesteric phase liquid crystal is formed will there be temperature response color change. Figure 3 As shown, it can be confirmed that a phase separation process occurs and spherical cholesteric liquid crystal is formed. Figure 4 As shown, by observing and counting the number of spherical cholesteric liquid crystals in each particle size range under POM, it can be seen that the particle size is mainly distributed between 80-130 um, with the majority being ~109 um, indicating that the particle size distribution is uniform, there is no agglomeration, and the size conforms to the normal distribution.

[0037] After testing, the reversible thermochromic film sample prepared in Example 1 can achieve reversible color change at 27-37°C, and appears colorless when the temperature is lower than 27°C or higher than 37°C. Figure 2 During the heating process, the absorption wavelength of the film is measured at three temperature points (27 ℃, 29 ℃, 36 ℃) in the color change range, which corresponds to the color visible to the naked eye at that temperature.

[0038] Embodiment 2:

[0039] A preparation method basically the same as that in Example 1 was adopted, with the only difference being that the rotation speeds of the five spin coating gradients in step 2 were different and the holding times of each stage were different, specifically: the spin coating speed of the first stage was 100 rpm, and the holding time was 50 s, the spin coating speed of the second stage was 200 rpm, and the holding time was 50 s, the spin coating speed of the third stage was 500 rpm, and the holding time was 50 s, the speed of the fourth stage was 15000 rpm, and the holding time was 50 s, and the speed of the fifth stage was 7000 rpm, and the holding time was 50 s, the amount of each spin coating was 250 μL, and the total coating thickness was 80 μm.

[0040] After testing, the response performance of the reversible thermochromic film sample prepared in Example 2 is equivalent to that in Example 1, and can achieve reversible color change between 27°C and 37°C, and display colorless when the temperature is lower than 27°C or higher than 37°C.

[0041] Comparative Example 1:

[0042] As a comparative experiment of Example 1, a preparation method substantially the same as that of Example 1 was adopted, the only difference being that the dissolution process in step S1 was stirred with a stirring bar (stirring speed of 1000 rpm for 0.5 h) with different parameters to form a transparent homogeneous solution.

[0043] POM (polarizing microscope) was used to observe the birefringence of liquid crystals to determine whether the final film contained liquid crystals, as well as the size, number, and morphology of the liquid crystals. Although liquid crystals were observed under POM in Comparative Example 1, the size of the liquid crystals was too small to form droplets (spherical), the color change was uneven, and the particle size was not uniform. By comparing with Example 1, it was proved that configuring the liquid crystals to form a homogeneous solution by appropriate stirring speed and time in the present invention is one of the keys to forming a reversible color-changing, spherical cholesteric liquid crystal film.

[0044] Comparative Example 2:

[0045] As a comparative experiment of Example 1, a preparation method substantially the same as that of Example 1 was adopted, with the only difference being that a scraping coating process was adopted in step S2, and the scraping coating thickness was fixed at 80 μm.

[0046] The film formed in Comparative Example 2 is light blue and has no temperature response color change. By observing under POM, liquid crystal exists, but only a small part of the liquid crystal forms cholesteric liquid crystal, and the naked eye cannot distinguish the color change, so there is no temperature response color change. By comparing with Example 1, it is proved that the gradient coating process used in the present invention is one of the keys to form a reversible color change, spherical cholesteric liquid crystal film.

[0047] Comparative Example 3:

[0048] As a comparative experiment of Example 1, a preparation method substantially the same as that of Example 1 was adopted, with the only difference being that a fixed temperature of 50° C. was used for drying in step S2, and the temperature had no gradient change.

[0049] In comparative example 3, drying at a fixed temperature results in the polymer being unable to wrap the liquid crystal, causing the liquid crystal to float on the surface. By observing under POM, when focusing on the film surface, the liquid crystal appears in clusters. After wiping with a paper towel, the film surface is observed again with POM, and no liquid crystal exists; when focusing on the inside of the film, only a small amount of liquid crystal exists. By comparing with Example 1, it is proved that the use of gradually increasing the temperature to dry the volatile solvent in the present invention is one of the keys to forming a reversible color-changing, spherical cholesteric liquid crystal film.

[0050] Comparative Example 4:

[0051] As a comparative experiment of Example 1, a preparation method substantially the same as that of Example 1 was adopted, with the only difference being that in step S2, the fourth and fifth stages of spin coating were omitted, and the total coating thickness was 80 μm by adjusting the first, second and third spin coating amounts.

[0052] The surface of the film formed in Comparative Example 4 is uneven and cannot be evenly spread over the entire substrate. Because the liquid crystal is unevenly distributed, some areas of the film change color in response to temperature, while some areas do not.

[0053] Comparative Example 5:

[0054] As a comparative experiment of Example 1, a preparation method substantially the same as that of Example 1 was adopted, with the only difference being that in step S2, the spin coating speed was gradually increased from an initial speed of 200 rpm to 7000 rpm at a fixed acceleration, the total time was 300 s, and the total coating thickness was 80 μm.

[0055] The spin coating speed of Comparative Example 5 has no step change, resulting in a white film surface. A large number of bubbles are observed under POM, and the color change cannot be distinguished by the naked eye, so there is no temperature response color change.

[0056] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film, It is characterized in that The following steps are involved: S1, using nematic liquid crystal and chiral liquid crystal as a liquid crystal mixture, dissolving the polylactic acid and liquid crystal mixture by a benign solution of the two to form a transparent homogeneous solution; S2, spin coating the homogeneous solution of step S1 on the substrate in a manner of increasing the spin coating speed from 50-200 rpm to 7000-8000 rpm, wherein each spin coating gradient is maintained for 30-90 s, and the spin coating thickness of each spin coating gradient is 5-25 μm; S3. After the spin coating is completed, the homogeneous solution spin-coated in step S2 is dried by gradually increasing the temperature, and a reversible thermochromic film is obtained after natural cooling.

2. The method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film according to claim 1, It is characterized in that In step S1, polylactic acid accounts for 70-99% of the total mass of the polylactic acid and liquid crystal mixture, the liquid crystal mixture accounts for 1-30% of the total mass of the polylactic acid and liquid crystal mixture; the nematic liquid crystal accounts for 50-99% of the total mass of the liquid crystal mixture, and the chiral agent accounts for 1-50% of the total mass of the liquid crystal mixture.

3. The method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film according to claim 1, It is characterized in that In step S1, the benign solution is one or a mixture of two or more of methanol, ethanol, isopropanol, acetone, dimethyl sulfoxide, dichloromethane, chloroform, acetonitrile, tetrahydrofuran, ethyl acetate, n-hexane, toluene, xylene, n-butanol, acetic acid, and pyridine.

4. The method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film according to claim 1, It is characterized in that The nematic phase liquid crystal is at least one of 4-cyano-4'-nonyloxybiphenyl, 4-cyano-4'-hexyloxybiphenyl, 4-cyano-4'-heptyloxybiphenyl, 4-cyano-4'-octyloxybiphenyl, 4-(4-cyanophenoxy)-4'-octylbiphenyl, and 4-cyano-4'-dodecylbiphenyl; the chiral agent liquid crystal is at least one of R5011, S5011, R811, and S811.

5. The method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film according to claim 1, It is characterized in that In step S1, a homogeneous solution is formed in the following manner: Add a stirrer to stir at a speed of 500-1500 rpm for 1-6 h; or shake on a shaker for 2-3 h; or clean in an ultrasonic cleaner at 40 kHz for 5 s-1 h.

6. The method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film according to claim 1, It is characterized in that In step S2, the spin coating speed is increased from 50-100 rpm to 7000-8000 rpm and is divided into at least three gradients.

7. The method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film according to claim 1, It is characterized in that In step S2, the spin coating speed is increased gradually in five stages, specifically: The spin coating speed of the first stage is 50-200 rpm, and the holding time is 50-60 s; the spin coating speed of the second stage is 200-500 rpm, and the holding time is 50-60 s; the spin coating speed of the third stage is 500-1000 rpm, and the holding time is 50-60 s; the speed of the fourth stage is 1500-3000 rpm, and the holding time is 50-60 s; the fifth stage is 7000 rpm, and the holding time is 50-60 s.

8. The method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film according to claim 1, It is characterized in that In step S3, the drying can be carried out by ultraviolet drying, infrared drying, hot air heating drying, and hot plate heating drying.

9. The method for preparing a simple, reversible thermochromic spherical cholesteric liquid crystal film according to claim 1, It is characterized in that In step S3, drying is performed at a heating rate of 5-10°C every 5 minutes from room temperature, and each 5-10°C heating period is maintained for 1-5 minutes.

10. A spherical cholesteric liquid crystal film prepared according to the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Temperature control dimming film based on ellipsoidal cholesteric liquid crystal micro-droplets and state transition method of temperature control dimming film

    CN111158179A

  • Preparation method of polymer dispersed liquid crystal film based on polymer nanofibers

    CN111736384A

  • Cholesteric liquid crystal elastomer composite film and preparation method thereof

    CN115449112A

  • Thermochromic cholesteric liquid crystal material and preparation method thereof

    CN116396743A

  • Multi-mode double-signal sensing film and preparation method thereof

    CN117901461A