Preparation method and application of natural fiber foaming material with buffering performance

By adding boric acid crosslinking agent and glycerin to the natural fiber solid solution, the buffering performance is improved, and the problems of poor buffering performance and toxic solvents of existing biomass-based buffering packaging materials are solved, and green and renewable buffering packaging materials are realized , suitable for large-scale manufacturing and application.

CN118978734APending Publication Date: 2024-11-19TIANJIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411306300.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing biomass-based buffer packaging materials have poor buffering performance and the organic solvents used are toxic, making it difficult to meet the needs of green and environmental protection.

Method used

By adding boric acid crosslinking agent and glycerin to the natural fiber solid solution, the hydroxyl crosslinking of boron ions and fibers is used to form a strong covalent combination, and the buffering performance is improved in synergistically, and toxic organic solvents are not used.

Benefits of technology

It significantly improves the buffering performance of natural fiber foamed materials, realizes low-cost, green and renewable buffer packaging materials, solves the pollution and waste problems of traditional packaging materials, and is suitable for large-scale manufacturing and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978734A_ABST
    Figure CN118978734A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of packaging materials, and particularly relates to a preparation method and application of a natural fiber foaming material with buffering performance, the preparation method comprises the following steps: adding water and a boric acid cross-linking agent into pulped natural fibers, mixing and stirring for cross-linking, then adding glycerol and a foaming agent, continuously stirring, pouring into a mold, and drying. The boric acid cross-linking agent is adopted for natural fiber cross-linking, through the synergistic effect of the added glycerin and the boric acid cross-linking agent, the buffer performance of the prepared natural fiber foaming material is improved, the buffer coefficient is 2-5, no organic solvent is used, and the natural fiber foaming material is green and environmentally friendly. The preparation process is simple, the reaction condition is mild and controllable, the operation is easy, the method is suitable for large-scale manufacturing, and the application prospect is wide. The natural fiber foaming material prepared by the method is applied to the field of paper-based packaging materials, finally made paper bags are simpler and lighter when applied to packaging, the pollution problem of existing packaging is solved, and the problem of complexity of the existing packaging is also solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of packaging materials and relates to a preparation method and application of a natural fiber foam material with cushioning performance. Background Art

[0002] In recent years, my country's express delivery industry has developed rapidly, and the number of express deliveries has increased year by year. However, the problems of express delivery packaging have also become increasingly prominent. The excessive use of a large number of express delivery packaging materials, low recycling rates, and improper handling not only waste resources, but also pollute the environment.

[0003] At present, express packaging mainly uses plastics, cartons, foam and other materials. Commonly used cushioning packaging now includes foamed plastic cushioning materials: but it consumes a lot of energy resources, the cost is uncontrollable, and it is easy to fluctuate; air cushion cushioning materials: too high or too low temperature will make its performance unstable and damage the items inside. Most of these cushioning materials are difficult to degrade, which puts great pressure on the environment. As society continues to improve its degree of environmental protection, people's environmental awareness is also gradually increasing. More and more consumers are beginning to pay attention to the impact of express packaging on the environment and choose to buy environmentally friendly packaging materials. At the same time, the government and enterprises also pay more attention to environmental protection work, promote the concepts of green logistics and green packaging, and urgently need to develop greener foaming materials to replace these petroleum-based foaming materials that are difficult to degrade and recycle.

[0004] Due to the unreasonable design of express packaging, a large amount of packaging materials are wasted. For example, the size of the carton is too large or too small, there is too much foam packaging, etc., which increases the consumption of packaging materials. Traditional express packaging can no longer meet the demand, and the innovation of packaging solutions has become necessary. Now many new technologies are beginning to be applied to the field of express packaging. For example, the research and development and promotion of degradable materials can reduce the impact on the environment while ensuring the packaging function. Natural fiber cushioning packaging materials are produced in recent years under the high international requirements for environmentally friendly green packaging materials. It is a degradable cushioning packaging foaming material. At present, it can be processed through biomass resources such as lignin, fiber, starch, etc., combined with the use of appropriate foaming agents and other related additives. It has the advantages of low cost, green environmental protection, recyclability and reuse, and has entered people's field of vision. Using paper bags instead of cartons can save packaging materials very well.

[0005] Chinese patent CN103992497A discloses a method for preparing biomass-based foam materials using natural fiber biomass materials, including: liquefaction conversion of biomass materials; synthesis of expandable resins; and foaming of synthetic resins. Although natural fibers are used, organic foaming agents and cross-linking agents are still required to achieve flame retardant, moisture-proof and heat-insulating properties, and the buffering properties need to be improved, and the organic solvents used are toxic.

[0006] Due to the poor cushioning performance of existing biomass-based cushioning packaging materials and the disadvantages that most materials are toxic, there is an urgent need to develop low-cost, good cushioning performance, and relatively green renewable resources for cushioning packaging. Summary of the invention

[0007] In order to solve the shortcomings of the above-mentioned prior art, the present invention provides a preparation method and application of a natural fiber foam material with cushioning properties. The method uses a boric acid cross-linking agent to cross-link the fibers, and adds glycerol and borax to synergistically improve the cushioning properties of the natural fiber foam material without using toxic organic solvents.

[0008] The technical solution adopted by the present invention to solve its technical problem is:

[0009] The first aspect of the present invention provides a method for preparing a natural fiber foam material with cushioning properties, the preparation method comprising:

[0010] A boric acid crosslinking agent is added to a solution containing 1.5-3 wt% of natural fiber solids, a basket grinding disperser is started, the speed of the disperser is adjusted to 2000-3000 r / min, and after stirring for 20-30 minutes, the speed of the disperser is slowly reduced to 200-300 r / min, glycerin and a foaming agent are added to the solution in sequence, and the speed of the disperser is gradually increased while the foaming agent is added until all the foaming agent is added and the speed of the disperser is increased to 2000-3000 r / min. After stirring for 10-20 minutes, a uniformly mixed wet foam can be obtained, the wet foam is poured into a mold and allowed to stand, filtered and shaped, and then placed in a blast drying oven at 40-80° C. and dried for 3-10 hours to obtain a natural fiber foam material; the cushioning coefficient of the natural fiber foam material is 2-5; the mass ratio of the natural fiber, the boric acid crosslinking agent, the glycerin, and the foaming agent is 4-6: 0.02-0.3: 2-3: 0.2-0.4.

[0011] Furthermore, the preparation method of the solution with a natural fiber solid content of 1.5 to 3 wt% is: soak the natural fibers in water for 5 to 10 hours, then beat them for 0.5 to 2 hours to obtain natural fibers with a beating degree of 20 to 65 SR°, and dry them to obtain absolutely dry natural fibers; add the absolutely dry natural fibers into water to prepare a solution with a natural fiber solid content of 1.5 to 3 wt%.

[0012] Furthermore, the natural fiber is one or more of hardwood, softwood, bamboo fiber, sugarcane fiber, and waste paper pulp.

[0013] Furthermore, the boric acid cross-linking agent is one or more of boric acid, borax and sodium borate.

[0014] Furthermore, the foaming agent is one or more of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide and Tween 80.

[0015] Furthermore, the filter mesh used for the water filtration and shaping is 80 meshes, and the water filtration time is 0.5 to 2 hours.

[0016] The second aspect of the present invention provides the use of the natural fiber foam material prepared by the preparation method in the preparation of paper-based packaging materials.

[0017] A third aspect of the present invention provides a paper-based packaging material prepared from the natural fiber foamed material prepared according to the preparation method.

[0018] A fourth aspect of the present invention provides a method for preparing the paper-based packaging material, comprising the following steps:

[0019] (1) Cutting the dried natural fiber foam material and laying it flat on the surface of kraft paper, controlling the height of the natural fiber foam material to be 3-5 mm, and bonding it to the kraft paper with an adhesive to obtain kraft paper with a foam layer as the sandwich; the natural fiber foam material is 60-200 g / m on the surface of the paper base. 2 ;

[0020] (2) Sealing the edges of the kraft paper with the foam layer sandwiched therein with edge sealing glue to obtain a complete kraft paper envelope bag paper;

[0021] (3) Cutting kraft paper envelope bag paper according to the paper pattern model of the paper bag, and finally using an edge banding machine to combine the model paper into kraft paper envelope bag paper to obtain paper-based packaging materials.

[0022] Furthermore, the adhesive is a mixture of styrene-butadiene latex, starch glue, starch glue and PVA in a certain proportion.

[0023] The advantages and positive effects achieved by the present invention are:

[0024] 1. The present invention adopts boric acid crosslinking agent to crosslink natural fibers. By adding glycerol and the synergistic effect of the boric acid crosslinking agent, the cushioning performance of the prepared natural fiber foaming material is improved, and no organic solvent is used, which is green and environmentally friendly.

[0025] 2. The preparation process of the natural fiber foam material of the present invention is simple, the reaction conditions are mild and controllable, it is easy to operate, suitable for large-scale production, and has broad application prospects.

[0026] 3. The natural fiber foam material prepared by the present invention is applied to the field of paper-based packaging materials, and is finally made into paper bags for use in packaging, which are simpler and lighter, and have a high degradation rate. This not only solves the pollution problem of existing packaging, but also solves the cumbersome problem of existing packaging.

[0027] 4. The present invention provides a stable and sustainable approach for the utilization of natural fiber foam materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The SEM images of the natural fiber foam materials prepared in Examples 1 to 6 of the present invention;

[0029] Figure 2 The following are the actual pictures of the natural fiber foam material prepared in Example 1 of the present invention and the actual pictures after being made into paper bags. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with the embodiments. The following embodiments are descriptive rather than restrictive, and the protection scope of the present invention cannot be limited by the following embodiments.

[0031] The various experimental operations involved in the specific embodiments are all routine techniques in the art. For parts not specially annotated in this document, ordinary technicians in the art can implement them by referring to various commonly used reference books, scientific and technological literature or related instructions, manuals, etc. before the filing date of this invention.

[0032] Example 1

[0033] A method for preparing a natural fiber foam material comprises the following steps:

[0034] The sugarcane fibers were soaked in water for 10 hours, and then beaten for 0.5 hours to obtain sugarcane fibers with a beating degree of 40 SR°, and then dried to obtain absolutely dry sugarcane fibers;

[0035] Add 5 g of absolutely dry sugarcane fiber with a beating degree of 40SR° into 250 mL of water to prepare a solution with a natural fiber solid content of 2 wt%, add 0.02 g of borax, start the basket grinder disperser, adjust the speed of the disperser to 2500 r / min, stir for 30 min, then slowly reduce the speed of the disperser to 300 r / min, add 2.5 g of glycerol and 0.3 g of sodium dodecyl sulfate in turn, gradually increase the speed of the disperser while adding the foaming agent, until all the foaming agent is added and the speed of the disperser is increased to 2500 r / min, stir for 15 min to obtain a uniformly mixed wet foam, pour the wet foam into a mold, let it stand and filter and set, the filter mesh is 80 mesh, the filter time is 1 h, put it in a blast drying oven at 45°C, and dry it for 5 h to obtain a natural fiber foam material.

[0036] The SEM image of the natural fiber foam material prepared in Example 1 is as follows: Figure 1 As shown in (a);

[0037] The method of preparing a paper-based packaging material using the natural fiber foaming material prepared in Example 1 comprises the following steps:

[0038] (1) Cut the dried natural fiber foam material and lay it flat on the surface of kraft paper, control the height of the natural fiber foam material to be 5 mm, and use starch glue to bond it to the kraft paper to obtain kraft paper with a foam layer in the middle; the natural fiber foam material is 90 g / m on the surface of the paper base; 2 ;

[0039] (2) Sealing the edges of the kraft paper with the foam layer sandwiched therein with edge sealing glue to obtain a complete kraft paper envelope bag paper;

[0040] (3) Cutting kraft paper envelope bag paper according to the paper pattern model of the paper bag, and finally using an edge banding machine to combine the model paper into kraft paper envelope bag paper to obtain paper-based packaging materials.

[0041] The actual picture of the prepared fiber foam material and the actual picture of the paper bag are as follows: Figure 2 As shown, it can be seen that the prepared paper bag is simple, light and easy to use.

[0042] Example 2

[0043] A method for preparing a natural fiber foam material comprises the following steps:

[0044] The sugarcane fibers were soaked in water for 10 hours, and then beaten for 1 hour to obtain sugarcane fibers with a beating degree of 50 SR°, and then dried to obtain absolutely dry sugarcane fibers;

[0045] 5 g of absolutely dry sugarcane fiber was added to 250 mL of deionized water to prepare a solution with a solid content of 2 wt%, 0.025 g of borax was added, the basket grinder was started, the speed of the disperser was adjusted to 2000 r / min, and after stirring for 20 min, the speed of the disperser was slowly reduced to 200 r / min, 2.5 g of glycerol and 0.3 g of sodium dodecyl sulfate were added thereto in sequence, and the speed of the disperser was gradually increased while adding the foaming agent until all the foaming agent was added and the speed of the disperser was increased to 3000 r / min. After stirring for 10 min, a uniformly mixed wet foam was obtained, and the wet foam was poured into a mold and allowed to stand for filtration and shaping. The filter mesh was 80 mesh and the filtration time was 1 h. The mixture was placed in a blast drying oven at 50° C. and dried for 5 h to obtain a natural fiber foam material.

[0046] The SEM image of the natural fiber foam material prepared in Example 2 is as follows: Figure 1 As shown in (b).

[0047] The method of preparing a paper-based packaging material using the natural fiber foaming material prepared in Example 2 comprises the following steps:

[0048] (1) Cut the dried natural fiber foam material and lay it flat on the surface of kraft paper, control the height of the natural fiber foam material to be 5 mm, and use starch glue to bond it to the kraft paper to obtain kraft paper with a foam layer in the middle; the natural fiber foam material is quantitatively 100 g / m on the surface of the paper base 2 ;

[0049] (2) Sealing the edges of the kraft paper with the foam layer sandwiched therein with edge sealing glue to obtain a complete kraft paper envelope bag paper;

[0050] (3) Cutting kraft paper envelope bag paper according to the paper pattern model of the paper bag, and finally using an edge banding machine to combine the model paper into kraft paper envelope bag paper to obtain paper-based packaging materials.

[0051] Example 3

[0052] A method for preparing a natural fiber foam material comprises the following steps:

[0053] The sugarcane fibers were soaked in water for 10 hours, and then beaten for 1 to 2 hours to obtain sugarcane fibers with a beating degree of 65 SR°, and then dried to obtain absolutely dry sugarcane fibers;

[0054] 5 g of absolutely dry sugarcane fiber was added to 250 mL of deionized water to obtain a solution with a solid content of 2%, and then 0.075 g of borax was added, and the basket grinder was started. The speed of the disperser was adjusted to 2500 r / min. After stirring for 30 minutes, the speed of the disperser was slowly reduced to 300 r / min, and 3 g of glycerol and 0.3 g of sodium dodecyl sulfate were added in sequence. While adding the foaming agent, the speed of the disperser was gradually increased until all the foaming agent was added and the speed of the disperser was increased to 2500 r / min. After stirring for 15 minutes, a uniformly mixed wet foam was obtained, which was poured into a mold and allowed to stand for filtration and shaping. The filter mesh was 80 mesh and the filtration time was 1 hour. The mixture was placed in a blast drying oven at 60°C and dried for 5 hours to obtain a natural fiber foam material.

[0055] The SEM image of the natural fiber foam material prepared in Example 3 is as follows: Figure 1 As shown in (c).

[0056] The method of preparing a paper-based packaging material using the natural fiber foaming material prepared in Example 3 comprises the following steps:

[0057] (1) Cut the dried natural fiber foam material and lay it flat on the surface of kraft paper, control the height of the natural fiber foam material to be 5 mm, and use starch glue to bond it to the kraft paper to obtain kraft paper with a foam layer in the middle; the natural fiber foam material is quantitatively 120 g / m on the surface of the paper base 2 ;

[0058] (2) Sealing the edges of the kraft paper with the foam layer sandwiched therein with edge sealing glue to obtain a complete kraft paper envelope bag paper;

[0059] (3) Cutting kraft paper envelope bag paper according to the paper pattern model of the paper bag, and finally using an edge banding machine to combine the model paper into kraft paper envelope bag paper to obtain paper-based packaging materials.

[0060] Example 4

[0061] A method for preparing a natural fiber foam material comprises the following steps:

[0062] 5 g of absolutely dry sugarcane fiber (same as in Example 1) with a beating degree of 40 SR° was weighed and added to 250 mL of deionized water to obtain a solution with a solid content of 2%. Then, 0.15 g of borax was added, and the basket grinder was started. The speed of the disperser was adjusted to 2500 r / min. After stirring for 30 min, the speed of the disperser was slowly reduced to 300 r / min. 2 g of glycerol and 0.3 g of sodium dodecyl sulfate were added thereto in sequence. While adding the foaming agent, the speed of the disperser was gradually increased until all the foaming agent was added and the speed of the disperser was increased to 2500 r / min. After stirring for 15 min, a uniformly mixed wet foam was obtained. The foam was poured into a mold and allowed to stand for filtration and shaping. The filter mesh was 80 mesh and the filtration time was 1 h. The foam was placed in a blast drying oven at 65° C. and dried for 5 h to obtain a natural fiber foam material.

[0063] The SEM image of the natural fiber foam material prepared in Example 4 is as follows: Figure 1 As shown in (d).

[0064] The method of preparing a paper-based packaging material using the natural fiber foaming material prepared in Example 4 comprises the following steps:

[0065] (1) Cut the dried natural fiber foam material and lay it flat on the surface of kraft paper, control the height of the natural fiber foam material to be 5 mm, and bond it to the kraft paper with starch glue to obtain kraft paper with a foam layer in the middle; the natural fiber foam material is quantitatively 150g / m on the surface of the paper base 2 ;

[0066] (2) Sealing the edges of the kraft paper with the foam layer sandwiched therein with edge sealing glue to obtain a complete kraft paper envelope bag paper;

[0067] (3) Cutting kraft paper envelope bag paper according to the paper pattern model of the paper bag, and finally using an edge banding machine to combine the model paper into kraft paper envelope bag paper to obtain paper-based packaging materials.

[0068] Example 5

[0069] A method for preparing a natural fiber foam material, the method comprising the following steps:

[0070] 5 g of absolute dry sugarcane fiber (same as in Example 2) with a beating degree of 50 SR° was weighed and added to 250 mL of deionized water to obtain a solution with a solid content of 2%. Then, 0.225 g of borax was added, and the basket grinding disperser was started. The speed of the disperser was adjusted to 2500 r / min. After stirring for 30 minutes, the speed of the disperser was slowly reduced to 300 r / min. 3 g of glycerol and 0.4 g of sodium dodecyl sulfate were added thereto in sequence. While adding the foaming agent, the speed of the disperser was gradually increased until all the foaming agent was added and the speed of the disperser was increased to 2500 r / min. After stirring for 15 minutes, a uniformly mixed wet foam was obtained. The foam was poured into a mold and allowed to stand for filtration and shaping. The filter mesh was 80 meshes and the filtration time was 1 hour. The foam was placed in a blast drying oven at 70° C. and dried for 5 hours to obtain a natural fiber foam material.

[0071] The SEM image of the natural fiber foam material prepared in Example 5 is as follows: Figure 1 As shown in (e).

[0072] The method of preparing a paper-based packaging material using the natural fiber foaming material prepared in Example 5 comprises the following steps:

[0073] (1) Cut the dried natural fiber foam material and lay it flat on the surface of kraft paper, control the height of the natural fiber foam material to be 5 mm, and use starch glue to bond it to the kraft paper to obtain kraft paper with a foam layer in the middle; the natural fiber foam material is 180 g / m on the surface of the paper base; 2 ;

[0074] (2) Sealing the edges of the kraft paper with the foam layer sandwiched therein with edge sealing glue to obtain a complete kraft paper envelope bag paper;

[0075] (3) Cutting kraft paper envelope bag paper according to the paper pattern model of the paper bag, and finally using an edge banding machine to combine the model paper into kraft paper envelope bag paper to obtain paper-based packaging materials.

[0076] Example 6

[0077] A method for preparing a natural fiber foam material, the method comprising the following steps:

[0078] 5 g of absolute dry sugarcane fiber (same as in Example 3) with a beating degree of 65 SR° was weighed and added to 250 mL of deionized water to obtain a solution with a solid content of 2%. Then, 0.3 g of borax was added, and the basket grinding disperser was started. The speed of the disperser was adjusted to 2500 r / min. After stirring for 30 minutes, the speed of the disperser was slowly reduced to 300 r / min. 2.5 g of glycerol and 0.3 g of sodium dodecyl sulfate were added thereto in sequence. While adding the foaming agent, the speed of the disperser was gradually increased until all the foaming agent was added and the speed of the disperser was increased to 2500 r / min. After stirring for 15 minutes, a uniformly mixed wet foam was obtained. The foam was poured into a mold and allowed to stand for filtration and shaping. The filter mesh was 80 mesh and the filtration time was 1 hour. The foam was placed in a blast drying oven at 80° C. and dried for 5 hours to obtain a natural fiber foam material.

[0079] The SEM image of the natural fiber foam material prepared in Example 6 is as follows: Figure 1 As shown in (f).

[0080] The method of preparing a paper-based packaging material using the natural fiber foaming material prepared in Example 6 comprises the following steps:

[0081] (1) Cut the dried natural fiber foam material and lay it flat on the surface of kraft paper, control the height of the natural fiber foam material to be 5 mm, and use starch glue to bond it to the kraft paper to obtain kraft paper with a foam layer in the middle; the natural fiber foam material is quantitatively 200 g / m on the surface of the paper base 2 ;

[0082] (2) Sealing the edges of the kraft paper with the foam layer sandwiched therein with edge sealing glue to obtain a complete kraft paper envelope bag paper;

[0083] (3) Cutting kraft paper envelope bag paper according to the paper pattern model of the paper bag, and finally using an edge banding machine to combine the model paper into kraft paper envelope bag paper to obtain paper-based packaging materials.

[0084] Comparative Example 1

[0085] The preparation method is the same as that of Example 1, except that glycerol is not added.

[0086] The natural fiber foaming material prepared in Comparative Example 1 was used to prepare a paper-based packaging material, and the preparation method was the same as that in Example 1.

[0087] Figure 1 The SEM images of the natural fiber foamed materials prepared in Examples 1 to 6 are as follows: the foamed material is taken with tweezers, and is pasted to a sample disk with conductive tape, and after gold spraying, the sample disk is placed in the sample chamber of a scanning electron microscope for observation and photography.

[0088] Table 1 shows the absorbed energy and buffering coefficient of the natural fibers prepared in Examples 1 to 6 of the present invention after foaming at 60% strain. The detection method is as follows: first, the experimental samples are pretreated in a constant temperature and humidity chamber for 24 hours. Referring to GB / T4875.2-2005 Packaging-Transport Package Test-Part 2: Temperature and Humidity Adjustment Treatment, the samples are pretreated at a constant temperature and humidity for 24 hours, with a temperature of 23°C and a relative humidity of 50%. The static compression test is carried out in accordance with the standard GBT 8168-2008 "Static Compression Test Method for Packaging Buffer Materials". The experimental equipment is an electronic material universal testing machine with a compression speed of 12mm / min and a compression strain of 60%. The stress-strain of the buffer material is obtained from the experiment. The number of measurements is three times. The absorbed energy of the natural fiber foam material can be calculated by integrating the stress-strain curve, and then the stress / absorbed energy is used as the buffering coefficient. The lowest point of the curve is usually used as the buffering coefficient of the material. Table 1 shows the absorbed energy, compressive strength and buffering coefficient of the natural fibers prepared in Examples 1 to 6 of the present invention and the comparative example after foaming at 60% strain.

[0089]

[0090] like Figure 1 It can be seen that the natural fiber foaming materials prepared in Examples 1 to 6 of the present invention have a porous structure and a high porosity, the fibers are cross-entangled with each other, and pores of different sizes are formed between the fibers. This is because the added boron ions cross-link with the hydroxyl groups of the fibers to form a strong covalent combination, and the addition of glycerol and borax produces a synergistic effect, which enhances the interaction between the fibers, thereby making the structural network more condensed. As can be seen from Table 1, Examples 1 to 6 have a small density, a large compressive strength, a high absorbed energy, and a small buffering coefficient, that is, the toughness of the material is improved, the extensibility of the material is improved, and the buffering effect is improved. Comparative Example 1 does not add glycerol, and the natural fiber prepared has a large density, a small compressive strength, a low absorbed energy value, and a high buffering coefficient. Without adding glycerol, the interaction between the fibers is weak, and the buffering performance is poor, indicating that glycerol and borax can synergistically enhance the interaction between the fibers, enhance the foam structure, and increase the buffering performance of the material. The paper-based packaging materials prepared in Examples 1 to 6 and Comparative Example 1 were tested for degradability, and the test data are shown in Table 2.

[0091] Table 2 Degradability test data of paper-based packaging materials prepared in Examples 1 to 6 and Comparative Example 1

[0092]

[0093] As can be seen from Table 2, in Examples 1 to 6, the addition of glycerol helps to further improve the degradability of the material. It promotes the biodegradation process of the material through synergistic effects with other ingredients, thereby reducing pollution to the environment and saving natural resources. In Comparative Example 1, where no glycerol was added, the 60-day degradation rate of the natural fiber decreased, indicating that glycerol can improve the mechanical properties of the fiber material and increase the toughness of the material, as well as plasticize and improve the fluidity of the material, which has a positive effect on the degradability of the fiber.

[0094] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.

Claims

1. A method for preparing a natural fiber foam material with cushioning properties, characterized in that: include: A boric acid crosslinking agent is added to a solution containing 1.5-3 wt% of natural fiber solids, a basket grinding disperser is started, the speed of the disperser is adjusted to 2000-3000 r / min, and after stirring for 20-30 minutes, the speed of the disperser is reduced to 200-300 r / min, glycerin and a foaming agent are added to the solution in sequence, and the speed of the disperser is gradually increased while the foaming agent is added until all the foaming agent is added, the speed of the disperser is increased to 2000-3000 r / min, and after stirring for 10-20 minutes, a uniformly mixed wet foam can be obtained, the wet foam is poured into a mold and allowed to stand, filtered and shaped, and then placed in a blast drying oven at 40-80° C. and dried for 3-10 hours to obtain a natural fiber foam material; the cushioning coefficient of the natural fiber foam material is 2-5; the mass ratio of the natural fiber, the boric acid crosslinking agent, the glycerin, and the foaming agent is 4-6: 0.02-0.3: 2-3: 0.2-0.

4.

2. The preparation method according to claim 1, characterized in that: The preparation method of the solution with a natural fiber solid content of 1.5 to 3 wt% is: soaking the natural fiber in water for 5 to 10 hours, then beating for 0.5 to 2 hours to obtain natural fiber with a beating degree of 20 to 65 SR°, and drying to obtain absolutely dry natural fiber; adding the absolutely dry natural fiber into water to prepare a solution with a natural fiber solid content of 1.5 to 3 wt%.

3. The preparation method according to claim 2, characterized in that: The natural fiber is one or more of hardwood, softwood, bamboo fiber, sugarcane fiber and waste paper pulp.

4. The preparation method according to claim 1, characterized in that: The boric acid cross-linking agent is one or more of boric acid, borax and sodium borate.

5. The preparation method according to claim 1, characterized in that: The foaming agent is one or more of sodium dodecyl sulfate, hexadecyl trimethyl ammonium bromide and Tween 80.

6. The preparation method according to claim 1, characterized in that: The filter mesh used for the water filtration and shaping is 80 meshes, and the water filtration time is 0.5 to 2 hours.

7. Use of the natural fiber foam material prepared by the preparation method according to any one of claims 1 to 6 in the preparation of paper-based packaging materials.

8. A paper-based packaging material made from the natural fiber foamed material prepared by the preparation method according to any one of claims 1 to 6.

9. The method for preparing a paper-based packaging material according to claim 8, characterized in that: The steps include: (1) Cutting the dried natural fiber foam material and laying it flat on the surface of kraft paper, controlling the height of the natural fiber foam material to be 3 to 5 mm, and bonding it to the kraft paper with an adhesive to obtain kraft paper with a foam layer as the sandwich; the natural fiber foam material is 60 to 200 g / m on the surface of the paper base. 2 ; (2) Sealing the edges of the kraft paper with the foam layer sandwiched therein with edge sealing glue to obtain a complete kraft paper envelope bag paper; (3) Cutting kraft paper envelope bag paper according to the paper pattern model of the paper bag, and finally using an edge banding machine to combine the model paper into kraft paper envelope bag paper to obtain paper-based packaging materials.