Composite treatment agent and method for sedimentation and transportation of oversize copper mine tailings

By using the combination of high acid ether ratio component A and polyacrylamide flocculants in copper tailings treatment, a dense flocculant structure is formed, which solves the problems of copper tailings settlement speed and transportation efficiency, and achieves high concentration and long distances Low energy consumption and delivery reduce drug consumption and energy consumption.

CN118978783AActive Publication Date: 2024-11-19CENT SOUTH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411040692.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The prior art is difficult to achieve efficient settlement and low energy consumption transportation in copper tailings treatment. Conventional flocculants cannot effectively solve the problems of slow settlement speed, inability to clarify overflow, and high bottom flow moisture content caused by increased fine particle content and degree of sludge. And improve the settlement efficiency and subsequent transmission efficiency and energy consumption.

Method used

Component A with a high acid ether ratio and polyether side chain combined with a polyacrylamide flocculant is used to provide a steric hinder effect through the carboxyl adsorption of component A and the electronegativity of the surface of the particles and the polyether side chain to form a steric hindrance effect. The dense floc structure increases the settlement speed and concentration bottom flow concentration, and enhances the slurry fluidity through the bridging of component B.

Benefits of technology

It significantly improves the settlement speed and concentration of copper tailings, improves the fluidity of slurry, reduces the energy consumption and chemical consumption of slurry transportation, realizes high-concentration, long-distance and low-energy consumption transportation, and improves tailings treatment efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978783A_ABST
    Figure CN118978783A_ABST
Patent Text Reader

Abstract

The invention discloses a composite treatment agent and method for sedimentation and conveying of oversize copper mine tailings, and belongs to the technical field of tailing treatment. The composite treatment agent comprises a molecular structure component A and a polyacrylamide component B: # imgabs0 #, wherein x / y is equal to (6-8): 1; n is 52-85, and R1 and R2 are independently selected from hydrogen or methyl. In the copper tailing slurry treatment process, a component A is adopted for adjusting copper tailings for interface regulation and control, then polypropylene is added for flocculation, micro-fine particles of the copper tailings are rapidly flocculated and settled to form dense and concentrated underflow, and the dense and concentrated underflow is conveyed to a tailing pond with low energy consumption. Meanwhile, ore pulp fluidity and conveying efficiency are improved, ore pulp conveying energy consumption and pipeline abrasion are reduced, the dosage of chemicals is small, and cost is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a composite treatment agent, in particular to a composite treatment agent used for settling and conveying of super-large copper mine tailings and a use method thereof, belonging to the technical field of tailings treatment. Background Art

[0002] Tailings are a large amount of solid waste generated after the selection of useful components in the process of mineral resource development and utilization. In the process of copper mining and beneficiation, 200 to 400 tons of copper tailings will be produced for every ton of copper concentrate produced. my country produces nearly 400 million tons of copper tailings each year, accounting for about 30% of the total tailings production in my country. It can be seen that the number of copper tailings is huge. If they are not properly handled scientifically, they will become a serious hidden danger to the ecological environment. In recent years, the mining of low-grade deposits has gradually increased. In order to achieve the full dissociation and efficient recovery of copper concentrate, copper ore is often ground to submicron size during the mineral sorting process, which also leads to an increase in fine particles in the tailings slurry. Therefore, the tailings slurry gradually forms a complex system with large quantity, fine particle size, low density, high viscosity and high mud content, which makes the treatment more difficult.

[0003] The treatment process of copper tailings includes the sedimentation, concentration, long-distance transportation of slurry and storage in tailings ponds. The conventional treatment method for copper tailings sedimentation is to add polymer flocculants. However, with the increase of fine particle content and muddiness of copper tailings slurry, conventional flocculants are also difficult to achieve efficient flocculation and sedimentation, exposing problems such as slow sedimentation rate, inability to clarify overflow, low bottom flow concentration / high water content. Therefore, coagulants such as inorganic salts and quaternary ammonium salt polyelectrolytes have been developed to cooperate with flocculants to increase the sedimentation rate of tailings and reduce the water content of bottom flow. However, most research works only aim to improve the sedimentation and concentration efficiency, without considering the impact on the subsequent long-distance transportation of tailings slurry, resulting in problems such as increased slurry viscosity and poor fluidity. Therefore, in the subsequent slurry transportation link, either the concentration of concentrated tailings is reduced by adding water, or the flocculant structure in the concentrated tailings is destroyed by adding agents to improve the slurry fluidity. These methods either increase the use of water and the energy consumption of tailings transportation, reduce the transportation efficiency, or increase the consumption of a large amount of chemicals, making the early efficient sedimentation and concentration unhelpful, greatly increasing the additional cost of tailings treatment.

[0004] Therefore, it is necessary to develop a multifunctional tailings treatment agent to achieve both efficient sedimentation and concentration of copper tailings and low-energy transportation of high-concentration tailings slurry, improve tailings treatment efficiency, and achieve sustainable development of mineral resource development. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, the first object of the present invention is to provide a composite treatment agent for the sedimentation and transportation of extra-large copper mine tailings. The composite treatment agent is used in the treatment process of extra-large copper tailings, which can increase the sedimentation rate and concentrated underflow concentration of copper tailings, improve the fluidity of the slurry, so as to achieve high-concentration, long-distance and low-energy transportation of copper tailings in subsequent links, thereby improving the overall efficiency of tailings treatment.

[0006] The second object of the present invention is to provide a method for settling and transporting extra-large copper mine tailings. The method uses a special composite treatment agent to improve the sedimentation rate of copper tailings and the concentration of concentrated underflow while improving the fluidity of the slurry, thereby achieving the purpose of improving the slurry transportation efficiency, reducing the energy consumption of slurry transportation and pipeline wear, reducing the amount of reagents used, and saving costs.

[0007] In order to achieve the above technical purpose, the present invention provides a composite treatment agent for settling and transporting super-large copper mine tailings, which comprises component A and component B;

[0008] The molecular structure of component A is as follows:

[0009]

[0010] in,

[0011] x / y=(6-8):1;

[0012] n = 52-85;

[0013] R 1 and R 2 are independently selected from hydrogen or methyl;

[0014] The component B is polyacrylamide.

[0015] The component A of the present invention has a high acid-ether ratio in its molecular structure, and uses its carboxyl group as an adsorption group to strengthen its neutralization effect on the electronegativity of the surface of the copper tailings particles, thereby weakening the electrostatic repulsion between the particles, making it easier for the particles to aggregate and settle quickly. At the same time, the component A has a high polyether side chain length, so that after the component A is adsorbed on the particle surface, it can not only provide a steric hindrance effect when flocs are formed, but also discharge water molecules in the floc space, thereby reducing the water content of the concentrated underflow and increasing the concentration of the concentrated underflow, and at the same time enhance the hydrophobicity of the particle surface, reduce the viscosity of the slurry, and increase the fluidity of the slurry, thereby improving the slurry transportation efficiency. In addition, the component A has a long main chain length, thereby improving its adsorption on the surface of the copper tailings particles, so that the effect of the coagulant on the sedimentation and transportation of the slurry is maximized.

[0016] The components A and B of the present invention have a synergistic effect in the process of treating copper tailings. The component A is adsorbed on the surface of the copper tailings particles, and the polyether side chains thereof are arranged in a direction toward the solution, so that the bridging effect of the component B on the particles is enhanced, and more fine particles in the ore pulp can be captured, thereby improving the clarity of the supernatant; the component A can compress the double electrical layer of the copper tailings particles, so that the component B forms a dense flocculent structure when bridging the copper tailings particles, thereby achieving the effect of improving the sedimentation velocity and the concentration of the concentrated underflow.

[0017] As a preferred embodiment, the weight average molecular weight M of component A is w =70,000 to 100,000.

[0018] As a preferred solution, the number average molecular weight Mn of the component B is 8 million to 12 million.

[0019] As a preferred solution, the composite treatment agent comprises the following components in parts by weight: 20 to 150 parts of component A; 2 to 8 parts of component B.

[0020] As a preferred solution, the polyacrylamide includes nonionic polyacrylamide and / or anionic polyacrylamide.

[0021] The present invention also provides a method for using the composite treatment agent for sedimentation and transportation of extra-large copper tailings, the method comprising adding component A in the composite treatment agent to copper tailings slurry for stirring pretreatment, adding component B in the composite treatment agent to the copper tailings slurry obtained by pretreatment, achieving rapid flocculation and sedimentation through thickening treatment to form a high-concentration concentrated underflow, and transporting the concentrated underflow to a tailings pond through a pipeline.

[0022] As a preferred solution, the dosage of component A in the copper ore tailings slurry is 200-1500 g / t.

[0023] As a preferred solution, the dosage of component B in the copper ore tailings slurry is 20-80 g / t.

[0024] As a preferred solution, the component A is added in the form of a solution with a mass concentration of 0.01 to 1.0%.

[0025] As a preferred solution, the component B is added in the form of a solution with a mass concentration of 0.005-0.1%.

[0026] As a preferred solution, during the stirring pretreatment process, the stirring speed is 200-400 r / min and the time is 10-20 min. Through the stirring action, component A can fully act on the surface of the copper tailings, realize the surface performance regulation of the copper tailings, and facilitate the subsequent flocculation and sedimentation process.

[0027] The preparation method of component A in the composite treatment agent for settling and transporting super-large copper mine tailings provided by the present invention mainly comprises the following steps, which are obtained by a conventional free radical polymerization method:

[0028] S1: Raw material preparation; the raw material components acrylic acid and / or methacrylic acid and methyl allyl alcohol polyoxyethylene ether are prepared in a molar ratio of (6-8):1; preferably, the molar ratio of acrylic acid and / or methacrylic acid to methyl allyl alcohol polyoxyethylene ether is (6.5-7):1; preferably, the molecular weight of methyl allyl alcohol polyoxyethylene ether is 2400-3800, more preferably 3000-3600, and its structural formula is as follows:

[0029]

[0030] S2: Reaction system construction; adding monomer raw materials into the reactor, and adding a certain amount of initiator and chain transfer agent in proportion; preferably, the initiator is any one of hydrogen peroxide, ammonium persulfate, and sodium persulfate, and the addition amount is 0.5-2.0% of the total mass of the monomer raw material, and more preferably 1.2-1.8%. By using a larger dose of initiator, the polymerization effect of the monomer raw material can be enhanced, so that the coagulant has a higher main chain length, thereby improving the adsorption of component A on the surface of copper tailings particles, maximizing its effect on slurry sedimentation and transportation; preferably, the chain transfer agent is a mixture of thioglycolic acid and mercaptopropionic acid in a mass ratio of 9:(1-3), and the addition amount is 0.3-0.8% of the total amount of the monomer raw material; more preferably, the mass ratio of the chain transfer agent thioglycolic acid to mercaptopropionic acid is 9:(1-1.5), and the addition amount is 0.3-0.6% of the total amount of the monomer raw material.

[0031] S3: polymerization reaction; at a certain temperature, the monomer raw material is polymerized by an initiator to form a high molecular chain polymer; preferably, the reaction temperature is 75 to 95° C., and more preferably, the reaction temperature is 90 to 95° C.; the reaction time is 2 to 4 hours, and more preferably, the reaction time is 3 to 3.5 hours;

[0032] S4: Neutralization treatment; after the polymerization reaction is completed, the high molecular chain polymer is neutralized to make its pH reach an ideal value to obtain a component A solution; preferably, the pH adjuster is sodium hydroxide, and the pH value is adjusted to 6.5-7.5.

[0033] The weight average molecular weight (M) of the component A product finally synthesized by the present invention is w) should be controlled in the range of 70,000 to 100,000, and more preferably in the range of 85,000 to 100,000. A higher molecular weight is helpful for the adsorption of two or more copper tailings particles. At the same time, the adsorption of the coagulant on the particle surface also helps the flocculant to bridge the particles, so that it can capture more fine particles in the slurry.

[0034] The method of using the composite treatment agent for sedimentation and transportation of extra-large copper tailings provided by the present invention is as follows: the copper tailings slurry first enters the pretreatment agitator, and component A with a mass concentration of 0.01 to 1.0% is continuously added to the pretreatment agitator to control the interface of the copper tailings; the pretreated slurry is pumped to the tailings thickener, and then a polyacrylamide flocculant with a mass concentration of 0.005 to 0.1% is continuously added to allow the copper tailings fine particles to quickly flocculate and settle in the thickener to form a high-concentration concentrated underflow; the concentrated underflow is then transported to the tailings pond via a long-distance pipeline. Preferably, the dosage of component A is 200 to 1500 g / t, and more preferably 500 to 1000 g / t. Preferably, the effective volume of the pretreatment agitator is 12 to 21 m 3 The further preferred effective volume is 15 to 18 m 3 , the stirring speed during the pretreatment process is 200-400r / min, and the further preferred stirring speed is 300-350r / min, the slurry residence time is 10-20min, and the further preferred residence time is 14-18min. In the present invention, the appropriate stirring speed and sufficient slurry residence time can make the particles in the slurry fully react and adsorb with the coagulant, reducing the consumption and excessive use of the agent. Preferably, the polyacrylamide is any one of nonionic polyacrylamide and anionic polyacrylamide, and more preferably nonionic polyacrylamide; the molecular weight of the polyacrylamide is in the range of 8 million to 12 million, and more preferably 10 million to 11 million; the dosage of the polyacrylamide is 20-80g / t, and the further preferred dosage is 30-65g / t, and more preferably 35-50g / t. The present invention adopts nonionic polyacrylamide to achieve better flocculation effect on copper tailings. The molecular weight of 10 million to 11 million can not only ensure the excellent flocculation ability of polyacrylamide, but also avoid that too high molecular weight of the agent will wrap water molecules in the flocs and affect the moisture content of the concentrated underflow.

[0035] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:

[0036] The key to the composite treatment agent for copper tailings sedimentation and transportation provided by the present invention is to use component A with a special molecular structure, and the main characteristics thereof are: on the one hand, a higher carboxylic acid ratio can neutralize the electronegativity of the particle surface and weaken the electrostatic repulsion between particles, thereby accelerating the sedimentation rate; on the other hand, a higher polyether side chain length can provide a steric hindrance effect, so that the formed flocs are denser and the concentrated underflow concentration is higher, and at the same time, the hydrophobicity of the particle surface can be enhanced, the slurry viscosity can be reduced, and the slurry fluidity and transportation efficiency can be improved; on the third aspect, a higher main chain length can improve the adsorption of the agent to the particles, maximize its effect on the sedimentation and transportation of the slurry, and reduce the agent consumption.

[0037] At present, the sedimentation treatment of super-large copper mine tailings adopts the method of using flocculants or coagulants in combination with flocculants. When conveying tailings, in order to improve fluidity, the pulp concentration needs to be reduced or rheological adjusters need to be added, which has the disadvantages of slow sedimentation rate, high water content of concentrated underflow, high transportation energy consumption, and large consumption of reagents. The present invention combines component A with a special molecular structure with polyacrylamide flocculants for copper mine tailings sedimentation and transportation, and has the following obvious technical advantages: 1. The sedimentation rate is better than the effect of the combination of traditional coagulants and flocculants, and the supernatant is clear; 2. The problem of high water content of concentrated underflow caused by flocculants is solved, and the concentration of concentrated underflow is significantly improved; 3. The pulp fluidity is greatly improved, and the tailings transportation does not need to reduce the pulp concentration or add other reagents, which saves transportation energy consumption and reagent costs, and realizes high-concentration, long-distance and low-energy transportation of super-large copper mine tailings. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is the Fourier transform infrared spectrum of component A in the composite treatment agent prepared in Example 1. DETAILED DESCRIPTION

[0039] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0040] Example 1

[0041] The sedimentation and transport performance test was carried out on the tailings of a large copper mine in Jiangxi. The main minerals in the tailings are quartz, chlorite and calcite, among which SiO 2 64.56%、Al 2 O 3 14.60%, pulp concentration 20.95%.

[0042] The preparation method of component A in the composite treatment agent is as follows: acrylic acid and methyl allyl alcohol polyoxyethylene ether with a molecular weight of 3200 are selected as monomer raw materials, and the ingredients are prepared in a molar ratio of 7:1 and added to a reactor; and ammonium persulfate initiator and a chain transfer agent with a mass ratio of thioglycolic acid to thiopropionic acid of 9:1 are added to the reactor respectively, and the addition amounts of the two additives are 1.5% and 0.5% of the total amount of the monomer raw materials, respectively; the reactor is heated to 95°C for polymerization reaction for 3.5 hours to form a high molecular chain polymer; after the reaction is completed, the high molecular chain polymer is neutralized with a sodium hydroxide pH adjuster, and the pH value is adjusted to 7.0 to obtain a component A solution.

[0043] The method of using the composite treatment agent for tailings sedimentation and transportation is as follows: the tailings slurry first enters the effective volume of 18m 3 A pretreatment agitator is provided, and component A with a mass concentration of 0.5% and a dosage of 1000g / t is continuously added into the pretreatment agitator to regulate the interface of the copper tailings. The stirring speed of the tailings slurry in the pretreatment agitator is 350r / min and the residence time is 18min; the pretreated slurry is then pumped to the tailings thickener, and a non-ionic polyacrylamide flocculant with a mass concentration of 0.025% and a dosage of 45g / t is continuously added, and its molecular weight is about 10 million, so that the fine particles of the copper tailings are quickly flocculated and settled in the thickener to form a high-concentration concentrated underflow; the concentrated underflow is then transported to the tailings pond through a 16km long-distance pipeline by pumping.

[0044] After testing, the weight average molecular weight of component A is 96700; the concentration of copper tailings underflow is 65.22%; and the apparent viscosity of the concentrated underflow at 300 rpm is 109.29 mPa·s.

[0045] Comparative Example 1

[0046] Other conditions were consistent with those in Example 1, except that the tailings slurry did not enter the pretreatment agitator, component A was not added for pretreatment, the tailings slurry was directly pumped to the tailings thickener, and a non-ionic polyacrylamide flocculant with a mass concentration of 0.025% and a dosage of 45 g / t was continuously added, and the molecular weight of the flocculant was about 10 million.

[0047] After testing, the copper tailings underflow concentration was 54.04%; the apparent viscosity of the concentrated underflow at 300 rpm was 133.76 mPa·s; compared with Example 1, the tailings transportation energy consumed was about 22.39% more.

[0048] Comparative Example 2

[0049] The other conditions are consistent with those in Example 1, except that: the tailings slurry enters the pretreatment agitator, and a traditional coagulant cetyltrimethylammonium bromide (CTAB) with a mass concentration of 0.5% and a dosage of 1500 g / t is continuously added to regulate the copper tailings interface; the pretreated slurry is then pumped to the tailings thickener, and a non-ionic polyacrylamide flocculant with a mass concentration of 0.025% and a dosage of 60 g / t is continuously added, and its molecular weight is about 10 million.

[0050] After testing, the copper tailings underflow concentration was 53.23%; the apparent viscosity of the concentrated underflow at 300 rpm was 135.14 mPa·s; compared with Example 1, the tailings transportation energy consumed was about 23.65% more.

[0051] Comparative Example 3

[0052] Other conditions are consistent with those in Example 1, except that: the tailings slurry enters the pretreatment agitator, and a traditional coagulant cetyltrimethylammonium bromide (CTAB) with a mass concentration of 1.0% and a dosage of 1800 g / t is continuously added to regulate the interface of the copper tailings; the pretreated slurry is then pumped to the tailings thickener, and a non-ionic polyacrylamide flocculant with a mass concentration of 0.025% and a dosage of 60 g / t is continuously added, and its molecular weight is about 17 million, so that the copper tailings are flocculated and settled in the thickener to form a concentrated underflow; the concentrated underflow is then pumped to the slurry mixing barrel, and an industrial-grade naphthalene-based water reducer with a mass concentration of 1.0% and a dosage of 2000 g / t is continuously added as a rheology adjuster; and the concentrated underflow is then transported to the tailings pond through a 16 km long-distance pipeline by pumping.

[0053] After testing, the copper tailings underflow concentration was 52.35%; the apparent viscosity of the concentrated underflow at 300 rpm was 126.02 mPa·s; compared with Example 1, the tailings transportation energy consumed was about 15.31% more.

[0054] Example 2

[0055] The difference from Example 1 is that in the preparation method of component A in the composite treatment agent, the monomer raw materials are methacrylic acid and methyl allyl alcohol polyoxyethylene ether with a molecular weight of 2400, and the other preparation methods are the same, and the use method of the composite treatment agent is the same.

[0056] After testing, the weight average molecular weight of component A is 83600; the concentration of copper tailings underflow is 64.39%; and the apparent viscosity of the concentrated underflow at 300 rpm is 111.45 mPa·s.

[0057] Comparative Example 4

[0058] Other conditions are consistent with those in Example 1, except that in the preparation method of component A in the composite treatment agent, methacrylic acid and isopentyl polyethylene glycol ether with a molecular weight of 1800 are selected as monomer raw materials, and other preparation methods are consistent, and the use method of the composite treatment agent is consistent.

[0059] After testing, the weight average molecular weight of component A is 65200; the copper tailings underflow concentration is 61.15%; the concentrated underflow apparent viscosity at 300rpm is 115.37mPa·s; compared with Example 2, the tailings transportation energy consumption is about 3.52% more.

[0060] Example 3

[0061] The difference from Example 1 is that in the preparation method of component A in the composite treatment agent, the monomer raw materials are acrylic acid and methyl allyl alcohol polyoxyethylene ether with a molecular weight of 3200, which are prepared in a molar ratio of 6:1 and added to the reactor. The other preparation methods are consistent, and the use method of the composite treatment agent is consistent.

[0062] After testing, the weight average molecular weight of component A is 92300; the concentration of copper tailings underflow is 64.56%; and the apparent viscosity of the concentrated underflow at 300 rpm is 110.46 mPa·s.

[0063] Comparative Example 5

[0064] Other conditions are consistent with those in Example 1, except that: in the preparation method of component A in the composite treatment agent, the monomer raw materials are acrylic acid and methyl allyl alcohol polyoxyethylene ether with a molecular weight of 3200, which are prepared in a molar ratio of 4:1 and added to the reactor. Other preparation methods are consistent, and the use method of the composite treatment agent is consistent.

[0065] After testing, the weight average molecular weight of component A is 80700; the copper tailings underflow concentration is 61.58%; the concentrated underflow apparent viscosity at 300rpm is 115.93mPa·s; compared with Example 3, the tailings transportation energy consumption is about 4.95% more.

[0066] Example 4

[0067] The difference from Example 1 is that in the preparation method of component A in the composite treatment agent, an ammonium persulfate initiator and a chain transfer agent with a mass ratio of thioglycolic acid to mercaptopropionic acid of 9:1 are added to the reactor, and the addition amounts of the two additives are 1.0% and 0.5% of the total amount of the monomer raw material, respectively; the reactor is heated to 85° C. for polymerization reaction for 3 hours to form a high molecular chain polymer, and the other preparation methods are consistent, and the use method of the composite treatment agent is consistent.

[0068] After testing, the weight average molecular weight of component A is 73500; the concentration of copper tailings underflow is 63.17%; and the apparent viscosity of the concentrated underflow at 300 rpm is 111.81 mPa·s.

[0069] Comparative Example 6

[0070] Other conditions are consistent with those in Example 1, except that: in the preparation method of component A in the composite treatment agent, ammonium persulfate initiator and thioglycolic acid chain transfer agent are added to the reactor respectively, and the addition amounts of the two additives are 0.3% and 0.5% of the total amount of monomer raw materials respectively; the reactor is heated to 85° C. to carry out polymerization reaction for 3 hours to form a high molecular chain polymer, and other preparation methods are consistent, and the use method of the composite treatment agent is consistent.

[0071] After testing, the weight average molecular weight of component A is 44600; the copper tailings underflow concentration is 58.19%; the concentrated underflow apparent viscosity at 300rpm is 119.64mPa·s; compared with Example 4, the tailings transportation energy consumption is about 7.01% more.

[0072] Example 5

[0073] The sedimentation and transportation performance test was carried out on the tailings of a large copper mine in Yunnan. The main minerals in the tailings are quartz, feldspar, chlorite and mica, among which SiO 2 56.88%, Al 2 O 3 13.20%, pulp concentration 22.46%.

[0074] The preparation method of component A in the composite treatment agent is as follows: acrylic acid and methyl allyl alcohol polyoxyethylene ether with a molecular weight of 3200 are selected as monomer raw materials, and the ingredients are prepared in a molar ratio of 7:1 and added to a reactor; and ammonium persulfate initiator and a chain transfer agent with a mass ratio of thioglycolic acid to thiopropionic acid of 9:1 are added to the reactor respectively, and the addition amounts of the two additives are 1.5% and 0.5% of the total amount of the monomer raw materials, respectively; the reactor is heated to 90°C for polymerization reaction for 3.5 hours to form a high molecular chain polymer; after the reaction is completed, the high molecular chain polymer is neutralized with a sodium hydroxide pH adjuster, and the pH value is adjusted to 7.0 to obtain a component A solution.

[0075] The method of using the composite treatment agent for tailings sedimentation and transportation is as follows: the tailings slurry first enters the effective volume of 21m 3A pretreatment agitator is provided, and component A with a mass concentration of 0.5% and a dosage of 750 g / t is continuously added into the pretreatment agitator to regulate the interface of the copper tailings. The stirring speed of the tailings slurry in the pretreatment agitator is 300 r / min and the residence time is 20 min. The pretreated slurry is then pumped to a tailings thickener, and an anionic polyacrylamide flocculant with a mass concentration of 0.025% and a dosage of 35 g / t is continuously added, and its molecular weight is 10 million to 11 million, so that the fine particles of the copper tailings can be quickly flocculated and settled in the thickener to form a high-concentration concentrated underflow. The concentrated underflow is then transported to the tailings pond through a 30 km long-distance pipeline by pumping.

[0076] After testing, the weight average molecular weight of component A is 93800; the concentration of copper tailings underflow is 64.93%; and the apparent viscosity of the concentrated underflow at 300 rpm is 110.48 mPa·s.

[0077] Comparative Example 7

[0078] The other conditions are consistent with those in Example 5, except that the pretreated slurry is pumped to the tailings thickener, and then a cationic polyacrylamide flocculant with a mass concentration of 0.025% and an addition amount of 35 g / t is continuously added, and the molecular weight of the cationic polyacrylamide flocculant is 11 million to 12 million. The use methods of other composite treatment agents are consistent, and the preparation method of component A is consistent.

[0079] After testing, the weight average molecular weight of component A is 93800; the copper tailings underflow concentration is 60.61%; the concentrated underflow apparent viscosity at 300rpm is 112.31mPa·s; compared with Example 5, the tailings transportation energy consumption is about 1.66% more.

[0080] Example 6

[0081] The sedimentation and transportation performance test was carried out using tailings from a large copper mine in Tibet. The main minerals in the tailings are quartz, mica, chlorite and, among which SiO 2 61.73%、Al 2 O 3 13.87%, pulp concentration 21.62%.

[0082] The preparation method of component A in the composite treatment agent is as follows: acrylic acid and methyl allyl alcohol polyoxyethylene ether with a molecular weight of 3200 are selected as monomer raw materials, and the ingredients are prepared in a molar ratio of 6.5:1 and added to a reactor; and ammonium persulfate initiator and a chain transfer agent with a mass ratio of thioglycolic acid to thiopropionic acid of 9:1 are added to the reactor respectively, and the addition amounts of the two additives are 1.5% and 0.5% of the total amount of the monomer raw materials respectively; the reactor is heated to 90°C for polymerization reaction for 3 hours to form a high molecular chain polymer; after the reaction is completed, the high molecular chain polymer is neutralized with sodium hydroxide pH adjuster, and the pH value is adjusted to 7.0 to obtain a component A solution.

[0083] The method of using the composite treatment agent for tailings sedimentation and transportation is as follows: the tailings slurry first enters the effective volume of 13.5m 3 A pretreatment agitator is provided, and component A with a mass concentration of 0.5% and a dosage of 800 g / t is continuously added into the pretreatment agitator to regulate the interface of the copper tailings. The stirring speed of the tailings slurry in the pretreatment agitator is 240 r / min and the residence time is 14 min; the pretreated slurry is then pumped to the tailings thickener, and an anionic polyacrylamide flocculant with a mass concentration of 0.025% and a dosage of 40 g / t is continuously added, and its molecular weight is 10 million to 11 million, so that the fine particles of the copper tailings can be quickly flocculated and settled in the thickener to form a high-concentration concentrated underflow; the concentrated underflow is then transported to the tailings pond through a 7 km long-distance pipeline by pumping.

[0084] After testing, the weight average molecular weight of component A is 93100; the concentration of copper tailings underflow is 64.62%; and the apparent viscosity of the concentrated underflow at 300 rpm is 109.75 mPa·s.

[0085] Comparative Example 8

[0086] The other conditions were consistent with those in Example 6, except that the stirring speed of the tailings slurry in the pretreatment agitator was 180 r / min, the residence time was 8 min, the use methods of other composite treatment agents were consistent, and the preparation method of component A was consistent.

[0087] After testing, the weight average molecular weight of component A is 93100; the copper tailings underflow concentration is 62.33%; the concentrated underflow apparent viscosity at 300rpm is 111.39mPa·s; compared with Example 6, the tailings transportation energy consumption is about 1.49% more.

[0088] In the present invention, the copper tailings slurry is pretreated by component A to increase the settling velocity of the tailings and the concentration of the concentrated underflow, while improving the fluidity of the concentrated underflow to reduce the transportation energy consumption. The specific manifestation of improving the fluidity is to reduce the apparent viscosity of the slurry. The transportation energy consumption of the slurry in the present invention is evaluated by the following formula.

[0089] The formula for calculating the energy consumption of slurry transportation is as follows:

[0090] E=P×t

[0091] Where: E—slurry transportation energy consumption, kWh

[0092] P—delivery pump power, kW

[0093] t—time, h

[0094] The calculation formula for the delivery pump is as follows:

[0095]

[0096] Where: P—delivery pump power, kW

[0097] ΔP—pressure drop provided by the delivery pump, Pa

[0098] Q—slurry volume flow rate, m3 / s

[0099] η P — Delivery pump efficiency

[0100] The pressure drop calculation formula when the slurry flows in the pipeline is as follows (Hagen-Poiseuille equation):

[0101]

[0102] Where: ΔP—pressure drop provided by the delivery pump, Pa

[0103] η—Paste viscosity, Pa·s

[0104] L—pipeline length, m

[0105] v—average slurry velocity, m / s

[0106] ρ—slurry density, kg / m3

[0107] d—pipe diameter, m

[0108] The above are only some of the preferred specific embodiments of the present invention and some of the cases in the process of technical exploration of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A composite treatment agent for sedimentation and transportation of extra-large copper mine tailings, Features: Comprising component A and component B; The molecular structure of component A is as follows: in, x / y=(6-8):1; n is 52 to 85; R 1 and R 2 are independently selected from hydrogen or methyl; The component B is polyacrylamide.

2. A composite treatment agent for settling and transporting super-large copper mine tailings according to claim 1, Features: The weight average molecular weight M of component A w =70,000 to 100,000; The number average molecular weight Mn of the component B is 8 million to 12 million.

3. A composite treatment agent for settling and transporting super-large copper mine tailings according to claim 1 or 2, Features: The composite treatment agent comprises the following components in parts by weight: 20 to 150 parts of component A; and 2 to 8 parts of component B.

4. A composite treatment agent for settling and transporting super-large copper mine tailings according to claim 1, Features: The polyacrylamides include nonionic polyacrylamide and / or anionic polyacrylamide.

5. A method for sedimentation and transportation of super-large copper mine tailings using the composite treatment agent according to any one of claims 1 to 4, Features: Component A in the composite treatment agent is added to copper tailings slurry for stirring pretreatment, and component B in the composite treatment agent is added to the copper tailings slurry obtained by pretreatment to achieve rapid flocculation and sedimentation through thickening treatment to form a high-concentration concentrated underflow, which is transported to the tailings pond through a pipeline.

6. The composite treatment agent according to claim 5 is used in the method for settling and transporting super-large copper mine tailings, Features: The dosage of component A in the copper ore tailings slurry is 200-1500 g / t; The dosage of component B in the copper ore tailings slurry is 20-80 g / t.

7. The composite treatment agent according to claim 6 is used in the method for settling and transporting super-large copper mine tailings, Features: The component A is added in the form of a solution with a mass concentration of 0.01 to 1.0%; The component B is added in the form of a solution with a mass concentration of 0.005-0.1%.

8. A method for settling and transporting super-large copper mine tailings using the composite treatment agent according to claim 5, 6 or 7, Features: During the stirring pretreatment process, the stirring speed is 200-400 r / min and the time is 10-20 min.

Citation Information

Patent Citations

  • Technology for treating scheelite mill tailings pulp by different steps through flocculation

    CN105903231A

  • Preparation method of phosphate water reducer with amide structure

    CN107964075A