Heat-resistant marine degradable injection molding packaging material
By combining polyhydroxy fatty acid esters with inorganic filler materials and cellulose for injection molding, and introducing epoxy soybean oil and hydroxyethyl methacrylate, the problem of insufficient brittleness and heat resistance of marine degraded injection molding packaging materials is solved. , achieving improved performance resistance, impact resistance and easy degradation.
Patent Information
- Application Number
- CN202411272643.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-17
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
AI Technical Summary
The existing marine degradation injection molded packaging materials have insufficient brittleness and heat resistance, resulting in deterioration of performance and limiting their application.
The melt plasticization and injection molding process is carried out using a mixture of polyhydroxy fatty acid esters, inorganic fillers, cellulose, antioxidants, anti-UV agents and lubricants, and the mechanical strength of the material is improved by the introduction of modified inorganic fillers and epoxy soybean oil. , thermal stability and biocompatibility, and enhance compatibility by hydroxyethyl methacrylate.
A heat-resistant, impact-resistant and easy-to-degradable marine degradation injection molded packaging material was prepared, which improved the mechanical strength and thermal stability of the material while maintaining environmentally friendly biodegradable properties.
Smart Images

Figure BDA0005039155440000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of material processing, and in particular discloses a heat-resistant marine degradable injection molding packaging material. Background Art
[0002] At present, packaging injection molding products are generally made of petroleum-based non-degradable plastics such as PP / PE / ABS, and degradable plastics are mainly PLA (polylactic acid) industrial composting degradation. However, these materials are no longer popular in Europe.
[0003] PHA (polyhydroxyalkanoate) is a general term for a class of intracellular bio-based polyesters with diverse structures synthesized by microbial fermentation. It is non-toxic and environmentally friendly. Compared with PLA, it is easier to process and degrade, and is very suitable for the preparation of packaging materials. However, PHA is brittle and its heat resistance needs to be improved. When it is directly added to polymers for modification, it has poor compatibility with the PHA matrix, resulting in performance degradation, which greatly limits its application. Therefore, it is of great significance to study a marine degradable injection molding packaging material with good toughness, good heat resistance and easy degradation. Summary of the invention
[0004] The object of the present invention is to provide a heat-resistant marine degradable injection molding packaging material to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A heat-resistant marine degradable injection molding packaging material, characterized in that the preparation of the marine degradable injection molding packaging material comprises the following steps:
[0007] Step 1: Mixing polyhydroxyalkanoate, inorganic filler, cellulose, antioxidant, anti-ultraviolet agent and lubricant to obtain a premix;
[0008] Step 2: Add the premix into the hopper of the parallel twin-screw extruder, melt and plasticize in the extruder, convey by screw pressure, extrude, and pelletize underwater to obtain pellets;
[0009] Step 3: The granular material is subjected to injection molding to obtain marine degradable injection molding packaging material.
[0010] Preferably, the mixing speed in step 1 is 400-900 rpm, and the mixing time is 10-30 min; the screw heating temperature used in step 2 is 150-195° C., the screw speed is 60-150 rpm, and the particle size of the granules is 3-5 mm; and the injection molding processing temperature in step 3 is 160-175° C., and medium pressure and medium speed injection molding.
[0011] Preferably, the premix comprises the following raw materials, by mass: 45-60 parts of polyhydroxyalkanoate, 5-15 parts of inorganic filler, 15-30 parts of cellulose, 0.1-0.5 parts of antioxidant, 0.1-0.5 parts of anti-ultraviolet agent, and 1-5 parts of lubricant.
[0012] Preferably, the polyhydroxyalkanoate includes one or more of polyhydroxybutyrate, polytrihydroxybutyrate, polytetrahydroxybutyrate, and copolyester of 3-hydroxybutyric acid and 3-hydroxyhexanoic acid.
[0013] Preferably, the inorganic filling material includes one or more of flaky talc, nano calcium sulfate, barium sulfate, and diatomaceous earth.
[0014] Preferably, the lubricant includes one or more low molecular weight lubricants selected from the group consisting of stearic acid, erucic acid, and polyethylene wax.
[0015] Preferably, the thickness of the marine degradable injection molding packaging material is 0.8-3 mm.
[0016] Preferably, the inorganic filling material is a modified inorganic filler, and the preparation method comprises the following steps: the preparation method comprises the following steps: take 3,3',5-trihydroxybiphenyl, triethylamine, flaky talc, diatomaceous earth, and acetonitrile, heat and stir under nitrogen protection, add ethyl acetate solution of epoxidized soybean oil, stir evenly, heat to react, filter to obtain the solid, wash, and dry to obtain the modified inorganic filler.
[0017] Preferably, the modified inorganic filler comprises the following raw materials, calculated by mass: 5 to 10 parts of 3,3',5-trihydroxybiphenyl, 8 to 12 parts of triethylamine, 20 to 30 parts of flaky talc, 20 to 30 parts of diatomaceous earth, and 400 to 500 parts of acetonitrile; the ethyl acetate solution of epoxidized soybean oil comprises the following raw materials, calculated by mass: 15 to 20 parts of epoxidized soybean oil and 150 to 250 parts of ethyl acetate.
[0018] Preferably, the premix further comprises 1 to 3 parts by mass of hydroxyethyl methacrylate.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: a modified inorganic filler is prepared, wherein the flaky talc and diatomaceous earth are used in combination to improve the mechanical strength, thermal stability and biocompatibility of polyhydroxyalkanoates; the present invention first introduces 3,3',5-trihydroxybiphenyl between the layers of flaky talc and diatomaceous earth, 3,3',5-trihydroxybiphenyl has a rigid ring structure, good heat resistance and high mechanical strength, and at the same time, the hydroxyl group provides a reaction site for the introduction of epoxy soybean oil in the next step, the introduction of epoxy soybean oil can improve the impact resistance and thermal stability of polyhydroxyalkanoates, and the epoxy soybean oil has good biocompatibility, does not affect the degradation of polyhydroxyalkanoates, and is environmentally friendly, wherein the epoxy group can also react with the hydroxyl group of cellulose in the subsequent process to improve the compatibility of the two; the present invention also adds hydroxyethyl methacrylate as a compatibilizer, one end of which can undergo an ester exchange reaction with the polyhydroxyalkanoate, and the hydroxyl group at the other end can react with the epoxy group of the epoxy soybean oil in the modified inorganic filler to improve the compatibility. DETAILED DESCRIPTION
[0020] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0021] The following parts are by mass unless otherwise specified;
[0022] Embodiment 1:
[0023] Step 1: Mixing polyhydroxyalkanoate, inorganic filler, cellulose, antioxidant, anti-ultraviolet agent and lubricant to obtain a premix;
[0024] Step 2: Add the premix into the hopper of the parallel twin-screw extruder, melt and plasticize in the extruder, convey by screw pressure, extrude, and pelletize underwater to obtain pellets;
[0025] Step 3: placing the pellets in an injection molding machine for injection molding to obtain marine degradable injection molding packaging materials;
[0026] The premix comprises the following raw materials, calculated by weight: 50 parts of polyhydroxyalkanoate, 15 parts of inorganic filler, 30 parts of cellulose, 0.25 parts of antioxidant, 0.25 parts of anti-ultraviolet agent, and 4.5 parts of lubricant;
[0027] The polyhydroxyalkanoate is polyhydroxybutyrate and polytrihydroxybutyrate and tetrahydroxybutyrate in a mass ratio of 1:1;
[0028] The inorganic filler material is flaky talc and diatomaceous earth in a mass ratio of 1:1;
[0029] The lubricant is erucamide;
[0030] In step one, the mixing speed is 500 rpm and the time is 20 min; in step two, the screw heating temperature used is 175°C, the screw speed is 120 rpm, and the particle size of the pellets is 4.0 mm; in step three, the injection molding process temperature range is 165°C, the pressure is medium pressure and medium speed injection molding, and the thickness of the marine degradable injection molding packaging material is 1 mm.
[0031] Embodiment 2: Step 1: Mix polyhydroxyalkanoate, inorganic filler, cellulose, antioxidant, anti-ultraviolet agent, hydroxyethyl methacrylate, and lubricant to obtain a premix;
[0032] Step 2: Add the premix into the hopper of the parallel twin-screw extruder, melt and plasticize in the extruder, convey by screw pressure, extrude, and pelletize underwater to obtain pellets;
[0033] Step 3: placing the pellets in an injection molding machine for injection molding to obtain marine degradable injection molding packaging materials;
[0034] The premix comprises the following raw materials, calculated by weight: 50 parts of polyhydroxyalkanoate, 15 parts of inorganic filler, 30 parts of cellulose, 0.25 parts of antioxidant, 0.25 parts of anti-ultraviolet agent, 4.5 parts of lubricant, and 2 parts of hydroxyethyl methacrylate;
[0035] The polyhydroxyalkanoate is polyhydroxybutyrate and polytrihydroxybutyrate and tetrahydroxybutyrate in a mass ratio of 1:1;
[0036] The inorganic filling material is a modified inorganic filler, and the preparation method comprises the following steps: taking 3,3',5-trihydroxybiphenyl, triethylamine, flaky talc, diatomaceous earth, and acetonitrile, heating and stirring to 45°C under nitrogen protection, stirring for 24 hours, adding an ethyl acetate solution of epoxy soybean oil, stirring evenly, stirring at 75°C for 14 hours, filtering and obtaining a solid, washing, and drying to obtain a modified inorganic filler;
[0037] The modified inorganic filler comprises the following raw materials, calculated by weight: 8 parts of 3,3',5-trihydroxybiphenyl, 10 parts of triethylamine, 25 parts of flaky talc, 25 parts of diatomaceous earth, and 450 parts of acetonitrile; the ethyl acetate solution of epoxy soybean oil comprises the following raw materials, calculated by weight: 18 parts of epoxy soybean oil and 200 parts of ethyl acetate;
[0038] The lubricant is erucamide;
[0039] In step one, the mixing speed is 500 rpm and the time is 20 min; in step two, the screw heating temperature used is 175°C, the screw speed is 120 rpm, and the particle size of the pellets is 4.0 mm; in step three, the injection molding process temperature range is 165°C, the pressure is medium pressure and medium speed injection molding, and the thickness of the marine degradable injection molding packaging material is 1 mm.
[0040] Embodiment 3: Step 1: Mix polyhydroxyalkanoate, inorganic filler, cellulose, antioxidant, anti-ultraviolet agent, lubricant, and hydroxyethyl methacrylate to obtain a premix;
[0041] Step 2: Add the premix into the hopper of the parallel twin-screw extruder, melt and plasticize in the extruder, convey by screw pressure, extrude, and pelletize underwater to obtain pellets;
[0042] Step 3: placing the pellets in an injection molding machine for injection molding to obtain marine degradable injection molding packaging materials;
[0043] The premix comprises the following raw materials, calculated by weight: 50 parts of polyhydroxyalkanoate, 15 parts of inorganic filler, 30 parts of cellulose, 0.25 parts of antioxidant, 0.25 parts of anti-ultraviolet agent, 4.5 parts of lubricant, and 3 parts of hydroxyethyl methacrylate;
[0044] The polyhydroxyalkanoate is polyhydroxybutyrate and polytrihydroxybutyrate and tetrahydroxybutyrate in a mass ratio of 1:1;
[0045] The inorganic filling material is a modified inorganic filler, and the preparation method comprises the following steps: taking 3,3',5-trihydroxybiphenyl, triethylamine, flaky talc, diatomaceous earth, and acetonitrile, heating and stirring to 45°C under nitrogen protection, stirring for 24 hours, adding an ethyl acetate solution of epoxy soybean oil, stirring evenly, stirring at 75°C for 14 hours, filtering and obtaining a solid, washing, and drying to obtain a modified inorganic filler;
[0046] The modified inorganic filler comprises the following raw materials, calculated by weight: 8 parts of 3,3',5-trihydroxybiphenyl, 10 parts of triethylamine, 25 parts of flaky talc, 25 parts of diatomaceous earth, and 450 parts of acetonitrile; the ethyl acetate solution of epoxy soybean oil comprises the following raw materials, calculated by weight: 18 parts of epoxy soybean oil and 200 parts of ethyl acetate;
[0047] The lubricant is erucamide;
[0048] In step 1, the mixing speed is 500 rpm and the time is 20 min. In step 2, the screw heating temperature used is 185°C, the screw speed is 120 rpm, and the particle size of the pellets is 4.0 mm. In step 3, the injection molding process temperature range is 175°C, the pressure is medium pressure and medium speed injection molding, and the thickness of the marine degradable injection molding packaging material is 1 mm.
[0049] Embodiment 4: Step 1: Mix polyhydroxyalkanoate, inorganic filler, cellulose, antioxidant, anti-ultraviolet agent, lubricant, and hydroxyethyl methacrylate to obtain a premix;
[0050] Step 2: Add the premix into the hopper of the parallel twin-screw extruder, melt and plasticize in the extruder, convey by screw pressure, extrude, and pelletize underwater to obtain pellets;
[0051] Step 3: placing the pellets in an injection molding machine for injection molding to obtain marine degradable injection molding packaging materials;
[0052] The premix comprises the following raw materials, calculated by weight: 50 parts of polyhydroxyalkanoate, 15 parts of inorganic filler, 30 parts of cellulose, 0.25 parts of antioxidant, 0.25 parts of anti-ultraviolet agent, 4.5 parts of lubricant, and 1 part of hydroxyethyl methacrylate;
[0053] The polyhydroxyalkanoate is polyhydroxybutyrate and polytrihydroxybutyrate and tetrahydroxybutyrate in a mass ratio of 1:1;
[0054] The inorganic filling material is a modified inorganic filler, and the preparation method comprises the following steps: taking 3,3',5-trihydroxybiphenyl, triethylamine, flaky talc, diatomaceous earth, and acetonitrile, heating and stirring to 45°C under nitrogen protection, stirring for 24 hours, adding an ethyl acetate solution of epoxy soybean oil, stirring evenly, stirring at 75°C for 14 hours, filtering and obtaining a solid, washing, and drying to obtain a modified inorganic filler;
[0055] The modified inorganic filler comprises the following raw materials, calculated by weight: 8 parts of 3,3',5-trihydroxybiphenyl, 10 parts of triethylamine, 25 parts of flaky talc, 25 parts of diatomaceous earth, and 450 parts of acetonitrile; the ethyl acetate solution of epoxy soybean oil comprises the following raw materials, calculated by weight: 18 parts of epoxy soybean oil and 200 parts of ethyl acetate;
[0056] The lubricant is erucamide;
[0057] In step 1, the mixing speed is 500 rpm and the time is 20 min. In step 2, the screw heating temperature used is 155°C, the screw speed is 120 rpm, and the particle size of the pellets is 4.0 mm. In step 3, the injection molding process temperature range is 175°C, the pressure is medium pressure and medium speed injection molding, and the thickness of the marine degradable injection molding packaging material is 1 mm.
[0058] Comparative Example 1 (hydroxyethyl methacrylate is not added, and the remaining method steps are consistent with Example 2): Step 1: Mix polyhydroxyalkanoate, inorganic filler material, cellulose, antioxidant, anti-ultraviolet agent, and lubricant to obtain a premix;
[0059] Step 2: Add the premix into the hopper of the parallel twin-screw extruder, melt and plasticize in the extruder, convey by screw pressure, extrude, and pelletize underwater to obtain pellets;
[0060] Step 3: placing the pellets in an injection molding machine for injection molding to obtain marine degradable injection molding packaging materials;
[0061] The premix comprises the following raw materials, calculated by weight: 50 parts of polyhydroxyalkanoate, 15 parts of inorganic filler, 30 parts of cellulose, 0.25 parts of antioxidant, 0.25 parts of anti-ultraviolet agent, and 4.5 parts of lubricant;
[0062] The polyhydroxyalkanoate is polyhydroxybutyrate and polytrihydroxybutyrate and tetrahydroxybutyrate in a mass ratio of 1:1;
[0063] The inorganic filling material is a modified inorganic filler, and the preparation method comprises the following steps: taking 3,3',5-trihydroxybiphenyl, triethylamine, flaky talc, diatomaceous earth, and acetonitrile, heating and stirring to 45°C under nitrogen protection, stirring for 24 hours, adding an ethyl acetate solution of epoxy soybean oil, stirring evenly, stirring at 75°C for 14 hours, filtering and obtaining a solid, washing, and drying to obtain a modified inorganic filler;
[0064] The modified inorganic filler comprises the following raw materials, calculated by weight: 8 parts of 3,3',5-trihydroxybiphenyl, 10 parts of triethylamine, 25 parts of flaky talc, 25 parts of diatomaceous earth, and 450 parts of acetonitrile; the ethyl acetate solution of epoxy soybean oil comprises the following raw materials, calculated by weight: 18 parts of epoxy soybean oil and 200 parts of ethyl acetate;
[0065] The lubricant is erucamide;
[0066] In step one, the mixing speed is 500 rpm and the time is 20 min; in step two, the screw heating temperature used is 175°C, the screw speed is 120 rpm, and the particle size of the pellets is 4.0 mm; in step three, the injection molding process temperature range is 165°C, the pressure is medium pressure and medium speed injection molding, and the thickness of the marine degradable injection molding packaging material is 1 mm.
[0067] Comparative Example 2 (the preparation method of the modified inorganic filler is changed, and the other method steps are consistent with Example 2): Step 1: Mix polyhydroxyalkanoate, inorganic filler material, cellulose, antioxidant, anti-ultraviolet agent, lubricant, and hydroxyethyl methacrylate to obtain a premix;
[0068] Step 2: Add the premix into the hopper of the parallel twin-screw extruder, melt and plasticize in the extruder, convey by screw pressure, extrude, and pelletize underwater to obtain pellets;
[0069] Step 3: placing the pellets in an injection molding machine for injection molding to obtain marine degradable injection molding packaging materials;
[0070] The premix comprises the following raw materials, calculated by weight: 50 parts of polyhydroxyalkanoate, 15 parts of inorganic filler, 30 parts of cellulose, 0.25 parts of antioxidant, 0.25 parts of anti-ultraviolet agent, 4.5 parts of lubricant, and 2 parts of hydroxyethyl methacrylate;
[0071] The polyhydroxyalkanoate is polyhydroxybutyrate and polytrihydroxybutyrate and tetrahydroxybutyrate in a mass ratio of 1:1;
[0072] The inorganic filling material is a modified inorganic filler, and the preparation method comprises the following steps: taking an ethyl acetate solution of 3,3',5-trihydroxybiphenyl, triethylamine, acetonitrile and epoxy soybean oil, stirring at 75°C under nitrogen protection for 24 hours, adding flaky talcum powder and diatomaceous earth, stirring for 12 hours, and removing the solvent to obtain a modified inorganic filler;
[0073] The modified inorganic filler comprises the following raw materials, calculated by weight: 8 parts of 3,3',5-trihydroxybiphenyl, 10 parts of triethylamine, 25 parts of flaky talc, 25 parts of diatomaceous earth, and 450 parts of acetonitrile; the ethyl acetate solution of epoxy soybean oil comprises the following raw materials, calculated by weight: 18 parts of epoxy soybean oil and 200 parts of ethyl acetate;
[0074] The lubricant is erucamide;
[0075] In step one, the mixing speed is 500 rpm and the time is 20 min; in step two, the screw heating temperature used is 175°C, the screw speed is 120 rpm, and the particle size of the pellets is 4.0 mm; in step three, the injection molding process temperature range is 165°C, the pressure is medium pressure and medium speed injection molding, and the thickness of the marine degradable injection molding packaging material is 1 mm.
[0076] Comparative Example 3 (the amount of flaky talc and diatomaceous earth added was changed, and the other method steps were consistent with Example 2): Step 1: polyhydroxyalkanoate, inorganic filler, cellulose, antioxidant, anti-ultraviolet agent, lubricant, and hydroxyethyl methacrylate were mixed to obtain a premix;
[0077] Step 2: Add the premix into the hopper of the parallel twin-screw extruder, melt and plasticize in the extruder, convey by screw pressure, extrude, and pelletize underwater to obtain pellets;
[0078] Step 3: placing the pellets in an injection molding machine for injection molding to obtain marine degradable injection molding packaging materials;
[0079] The premix comprises the following raw materials, calculated by weight: 50 parts of polyhydroxyalkanoate, 15 parts of inorganic filler, 30 parts of cellulose, 0.25 parts of antioxidant, 0.25 parts of anti-ultraviolet agent, 4.5 parts of lubricant, and 2 parts of hydroxyethyl methacrylate;
[0080] The polyhydroxyalkanoate is polyhydroxybutyrate and polytrihydroxybutyrate and tetrahydroxybutyrate in a mass ratio of 1:1;
[0081] The inorganic filling material is a modified inorganic filler, and the preparation method comprises the following steps: taking 3,3',5-trihydroxybiphenyl, triethylamine, flaky talc, diatomaceous earth, and acetonitrile, heating and stirring to 45°C under nitrogen protection, stirring for 24 hours, adding an ethyl acetate solution of epoxy soybean oil, stirring evenly, stirring at 75°C for 14 hours, filtering and obtaining a solid, washing, and drying to obtain a modified inorganic filler;
[0082] The modified inorganic filler comprises the following raw materials, calculated by weight: 8 parts of 3,3',5-trihydroxybiphenyl, 10 parts of triethylamine, 5 parts of flaky talc, 45 parts of diatomaceous earth, and 450 parts of acetonitrile; the ethyl acetate solution of epoxy soybean oil comprises the following raw materials, calculated by weight: 18 parts of epoxy soybean oil and 200 parts of ethyl acetate;
[0083] The lubricant is erucamide;
[0084] In step one, the mixing speed is 500 rpm and the time is 20 min; in step two, the screw heating temperature used is 175°C, the screw speed is 120 rpm, and the particle size of the pellets is 4.0 mm; in step three, the injection molding process temperature range is 165°C, the pressure is medium pressure and medium speed injection molding, and the thickness of the marine degradable injection molding packaging material is 1 mm.
[0085] Comparative Example 4 (phenylphosphonic acid dichloride is used instead of epoxy soybean oil, and the other method steps are consistent with Example 2): Step 1: polyhydroxyalkanoate, inorganic filler material, cellulose, antioxidant, anti-ultraviolet agent, lubricant, and hydroxyethyl methacrylate are mixed to obtain a premix;
[0086] Step 2: Add the premix into the hopper of the parallel twin-screw extruder, melt and plasticize in the extruder, convey by screw pressure, extrude, and pelletize underwater to obtain pellets;
[0087] Step 3: placing the pellets in an injection molding machine for injection molding to obtain marine degradable injection molding packaging materials;
[0088] The premix comprises the following raw materials, calculated by weight: 50 parts of polyhydroxyalkanoate, 15 parts of inorganic filler, 30 parts of cellulose, 0.25 parts of antioxidant, 0.25 parts of anti-ultraviolet agent, 4.5 parts of lubricant, and 2 parts of hydroxyethyl methacrylate;
[0089] The polyhydroxyalkanoate is polyhydroxybutyrate and polytrihydroxybutyrate and tetrahydroxybutyrate in a mass ratio of 1:1;
[0090] The inorganic filling material is a modified inorganic filler, and the preparation method comprises the following steps: taking 3,3',5-trihydroxybiphenyl, triethylamine, flaky talc, diatomaceous earth, and acetone, heating and stirring to 45°C under nitrogen protection, stirring for 24 hours, adding an acetone solution of phenylphosphonic dichloride, stirring for 12 hours, filtering and obtaining a solid, washing, and drying to obtain a modified inorganic filler;
[0091] The modified inorganic filler comprises the following raw materials, calculated by weight: 8 parts of 3,3',5-trihydroxybiphenyl, 10 parts of triethylamine, 25 parts of flaky talc, 25 parts of diatomaceous earth, and 450 parts of acetone; the acetone solution of epoxy soybean oil comprises the following raw materials, calculated by weight: 18 parts of phenylphosphonic dichloride and 200 parts of acetone;
[0092] The lubricant is erucamide;
[0093] In step one, the mixing speed is 500 rpm and the time is 20 min; in step two, the screw heating temperature used is 175°C, the screw speed is 120 rpm, and the particle size of the pellets is 4.0 mm; in step three, the injection molding process temperature range is 165°C, the pressure is medium pressure and medium speed injection molding, and the thickness of the marine degradable injection molding packaging material is 1 mm.
[0094] In the above embodiments, the test methods used are conventional methods unless otherwise specified; the raw materials used are commercially available unless otherwise specified, and the sources of the raw materials are as follows: polyhydroxybutyrate (MDF1000, Zhuhai Maidefa Biotechnology Co., Ltd.), polytrihydroxybutyrate tetrahydroxybutyrate (MDF1500, Zhuhai Maidefa Biotechnology Co., Ltd.); 3,3',5-trihydroxybiphenyl (CAS: 20950-56-5); triethylamine (CAS: 121-44-8); acetone (CAS: 67-64-1); epoxidized soybean oil (S50881, Shanghai Yuanye); ethanol (CAS: 64-17-5 ); hydroxyethyl methacrylate (CAS: 868-77-9); acetonitrile (CAS: 75-05-8); ethyl acetate (CAS: 141-78-6); phenylphosphonic acid dichloride (CAS: 824-72-6); flaky talc (LP-H01, Zhongshan Laipeng New Materials Co., Ltd.); diatomaceous earth (HG173, Mantanghong); erucic acid amide (Y20561, Shanghai Yuanye); cellulose (XK1439, Hubei Xinkang Pharmaceutical Chemical Co., Ltd.); antioxidant (trioctyl trimellitate, B67050, Shanghai Yuanye); anti-ultraviolet agent (ultraviolet absorber UV-531, Nanjing Milan New Materials Co., Ltd.).
[0095] Experiment: Take the marine degradable injection molding packaging materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4; (1) detect the degradation time of marine degradation; (2) refer to GB / T 1843-2008 to detect the impact strength; (3) refer to GB / T 1634.2 to detect the heat deformation temperature; the specific data are shown in the table below;
[0096]
[0097] Conclusion: From the above table, compared with Example 2, Comparative Example 1 did not add hydroxyethyl methacrylate, and the performance decreased due to the change in the compatibility of the modified inorganic filler, cellulose, and polyhydroxyalkanoate; Comparative Example 2 changed the preparation method of the modified inorganic filler, first compounded 3,3',5-trihydroxybiphenyl and epoxy soybean oil, and then added flaky talcum powder and diatomaceous earth, resulting in a decrease in performance; Comparative Example 3 changed the amount of flaky talcum powder and diatomaceous earth added, resulting in performance not as good as the embodiment, from which it can be seen that controlling the amount of flaky talcum powder and diatomaceous earth added is of great significance; Comparative Example 4 used phenylphosphonic dichloride instead of epoxy soybean oil, and the impact strength was significantly reduced, and it was not easy to degrade. In summary, the marine degradable injection molding packaging material prepared by the present invention is heat-resistant, impact-resistant, and easy to degrade.
[0098] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A heat-resistant marine degradable injection molding packaging material, characterized in that: The preparation of the marine degradable injection molding packaging material comprises the following steps: Step 1: Mixing polyhydroxyalkanoate, inorganic filler, cellulose, antioxidant, anti-ultraviolet agent and lubricant to obtain a premix; Step 2: melt and plasticize the premix, convey it by screw pressure, extrude it, and pelletize it underwater to obtain pellets; Step 3: The granular material is subjected to injection molding to obtain marine degradable injection molding packaging material.
2. The heat-resistant marine degradable injection molding packaging material according to claim 1, characterized in that: The premix comprises the following raw materials, calculated by weight: 45-60 parts of polyhydroxyalkanoate, 5-15 parts of inorganic filler, 15-30 parts of cellulose, 0.1-0.5 parts of antioxidant, 0.1-0.5 parts of anti-ultraviolet agent, and 1-5 parts of lubricant.
3. The heat-resistant marine degradable injection molding packaging material according to claim 1, characterized in that: The polyhydroxyalkanoate includes one or more of polyhydroxybutyrate, polytrihydroxybutyrate, polytetrahydroxybutyrate, and copolyester of 3-hydroxybutyric acid and 3-hydroxycaproic acid.
4. The heat-resistant marine degradable injection molding packaging material according to claim 1, characterized in that: The inorganic filling material includes one or more of flaky talc, nano calcium sulfate, barium sulfate, and diatomaceous earth.
5. The heat-resistant marine degradable injection molding packaging material according to claim 1, characterized in that: The lubricant includes one or more low molecular weight lubricants such as stearic acid, erucic acid, and polyethylene wax.
6. The heat-resistant marine degradable injection molding packaging material according to claim 1, characterized in that: The thickness of the marine degradable injection molding packaging material is 0.8-3 mm.
7. The heat-resistant marine degradable injection molding packaging material according to claim 1, characterized in that: The inorganic filling material is a modified inorganic filler, and the preparation method comprises the following steps: taking 3,3',5-trihydroxybiphenyl, triethylamine, flaky talc, diatomaceous earth, and acetonitrile, heating and stirring under nitrogen protection, adding ethyl acetate solution of epoxy soybean oil, stirring evenly, heating to react, filtering to obtain a solid, washing, and drying to obtain a modified inorganic filler.
8. The heat-resistant marine degradable injection molding packaging material according to claim 7, characterized in that: The modified inorganic filler includes the following raw materials, calculated by mass: 5 to 10 parts of 3,3',5-trihydroxybiphenyl, 8 to 12 parts of triethylamine, 20 to 30 parts of flaky talc, 20 to 30 parts of diatomaceous earth, and 400 to 500 parts of acetonitrile; the ethyl acetate solution of epoxidized soybean oil includes the following raw materials, calculated by mass: 15 to 20 parts of epoxidized soybean oil and 150 to 250 parts of ethyl acetate.
9. The heat-resistant marine degradable injection molding packaging material according to claim 1, characterized in that: The premix further comprises 1 to 3 parts of hydroxyethyl methacrylate by weight.