Microencapsulated gardenia yellow pigment and preparation method thereof

The pH-responsive microcapsules were constructed by co-embedding polymers, which solved the problem of gardenia yellow being easily browned in acidic environments, achieved stability under acidic conditions and rapid release under alkaline conditions, and extended service life And improves the UV resistance.

CN118978815AInactive Publication Date: 2024-11-19HENAN ZHONGDA HENGYUAN BIOTECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411052789.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Gardenia yellow is prone to browning in an acidic environment, which damages the color and durability of the product and limits its application range.

Method used

Using co-embedded polymer as the microcapsule wall material, the pH responsiveness of polyvinylpyridine and the UV resistance of modified methyl methacrylate are constructed to slow down the release rate under acidic conditions and improve stability. Sex and service life.

Benefits of technology

Under acidic conditions, the release rate of gardenia yellow is slowed down, the color stability is maintained, and the release rate is accelerated under alkaline conditions, extending service life, and improving the resistance to ultraviolet rays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004975418540000041
    Figure BDA0004975418540000041
  • Figure BDA0004975418540000051
    Figure BDA0004975418540000051
  • Figure BDA0004975418540000101
    Figure BDA0004975418540000101
Patent Text Reader

Abstract

The invention discloses a microencapsulated gardenia yellow pigment and a preparation method thereof, and relates to the technical field of gardenia yellow pigment microcapsules. The gardenia yellow pigment is subjected to microencapsulation treatment by adopting a co-embedded polymer as a microcapsule wall material, and the gardenia yellow pigment is relatively good in light resistance and heat resistance under a neutral or slightly alkaline condition, but is relatively poor in heat resistance and light resistance and easy to brown at a low pH value, so that the problem that the gardenia yellow pigment is prone to browning under an acidic condition is avoided. Compared with the prior art, the preparation method has the advantages that the pH-responsive microcapsule is constructed by adopting a co-embedded polymer, so that the release speed of the pH-responsive microcapsule is slowed down or stopped under an acidic condition, but the release speed of the pH-responsive microcapsule is accelerated under an alkaline condition, and therefore, polyvinyl pyridine is adopted as a release switch, is an alkalescent polymer, is ionized at medium and low pH values, and is protonized at a high pH value; therefore, the intermolecular gap is enlarged, and then the release speed is accelerated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gardenia yellow pigment microcapsules, in particular to microencapsulated gardenia yellow pigment and a preparation method thereof. Background Art

[0002] Gardenia yellow, also known as crocin, commonly known as yellow gardenia, is a natural pigment belonging to the carotenoid series. It is derived from the fruit of gardenia, and its main yellow component is the same as the crocin contained in saffron, both of which are carotenoid pigments. Gardenia yellow has a wide range of applications in the food industry due to its bright yellow hue. It is often used in the processing and production of a variety of foods such as fruit juice (flavored) drinks, blended wines, decorative makeup on the surface of pastries, popsicles, ice cream, puffed foods, jellies, cakes, candies, and canned chestnuts, adding bright colors to these products.

[0003] However, the chemical stability of Gardenia Yellow is significantly affected by the pH value of the environment. Under neutral or alkaline conditions, Gardenia Yellow exhibits good light and heat resistance, and can maintain its bright color without fading or deterioration. However, in an acidic environment with a low pH value, its heat and light resistance are greatly reduced, and it is easy to brown, which not only damages the appearance and color of the product, but also limits the application of Gardenia Yellow in certain acidic environments.

[0004] Therefore, in order to expand the application scope of Gardenia Yellow, especially its use in acidic environments, researchers are committed to developing a microcapsule technology. This technology aims to encapsulate Gardenia Yellow through microcapsules, so that it can be released quickly in alkaline environments and released more slowly in acidic conditions, thereby effectively protecting Gardenia Yellow from the effects of acidic environments, maintaining its color stability and extending its service life. Summary of the invention

[0005] The object of the present invention is to provide a microencapsulated gardenia yellow pigment and a preparation method thereof, so as to solve the problems existing in the prior art.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A method for preparing microencapsulated gardenia yellow pigment, wherein the microencapsulated gardenia yellow pigment is prepared by the following steps:

[0008] S1. Under nitrogen protection, add pretreated polyethylene glycol monomethyl ether, vinyl pyridine, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:3.8-4.1:0.08-0.09:0.06-0.08, stir evenly, freeze and vacuumize with liquid nitrogen, fill with nitrogen to thaw 2-3 times, stir at 25-30°C for 25-35min, heat to 55-65°C after stirring for 8-12h, add tetrahydrofuran 3-4 times the mass of pretreated polyethylene glycol monomethyl ether after the reaction is completed, stir evenly and dilute to stop the reaction, remove copper ions from an alumina chromatography column, and concentrate the solution after passing through the chromatography column by rotary evaporation. After rotary evaporation and concentration, add 3-5 times the mass of n-hexane of the remaining solution and let it settle, filter after settling, and vacuum dry the filtered product to obtain a preliminary co-embedded product;

[0009] S2. Under nitrogen protection, add the preliminary co-embedded product, modified methyl methacrylate, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:24-26:1.8-2.2:0.15-0.18, stir evenly, freeze and evacuate with liquid nitrogen, fill with nitrogen to thaw 2-3 times, stir at 25-30°C for 25-35min, heat to 55-65°C after stirring for 8-12h, add tetrahydrofuran 3-4 times the mass of the preliminary co-embedded product after the reaction is completed, stir evenly to dilute and stop the reaction, remove the copper ions by an alumina chromatography column, and concentrate the solution after passing through the chromatography column by rotary evaporation. After rotary evaporation and concentration, add 3-5 times the mass of n-hexane of the remaining solution and let it settle, filter after settling, and vacuum dry the filtered product to obtain a co-embedded polymer;

[0010] S3. Add the co-embedded polymer to dichloromethane at a mass ratio of 1:50-60, stir to dissolve, then add 0.6-0.8 times the mass of the co-embedded polymer, and ultrasonically disperse for 20-25 minutes to obtain an oil phase; add the oil phase to the aqueous phase at a volume ratio of 1:1 at a temperature of 25-30°C, stir for 3-5 minutes at a speed of 1800 rpm, and then stir for 4-6 hours at a speed of 600 rpm, let stand to evaporate and remove the organic solvent, then perform ultrafiltration and centrifugation, and wash the centrifuged product with deionized water for 2-3 times, and freeze-dry to obtain microencapsulated gardenia yellow pigment.

[0011] As an optimization, the water phase in S3 is a polyvinyl alcohol aqueous solution with a mass fraction of 0.4%.

[0012] As an optimization, the pretreated polyethylene glycol monomethyl ether in S1 is prepared according to the following method: triethylamine is added to tetrahydrofuran at a mass ratio of 1:80-90, and the mixture is stirred evenly to prepare a triethylamine solution for standby use; 2-bromoisobutyryl bromide is added to tetrahydrofuran at a mass ratio of 1:120-130, and the mixture is stirred evenly to prepare a 2-bromoisobutyryl bromide solution for standby use; at a temperature of 0-5°C, polyethylene glycol monomethyl ether is added to toluene at a mass ratio of 1:3.5-3.8, the mixture is stirred evenly, and a triethylamine solution 3.5-3.7 times the mass of polyethylene glycol monomethyl ether is added, and after mixing evenly, a uniform rate of dripping is added within 2-2.5 hours. After the dropwise addition of 2-bromoisobutyryl bromide solution with a mass of 1.1 to 1.3 times of the mass of polyethylene glycol monomethyl ether is completed, the reaction is stirred for 36 to 48 hours at a temperature of 25 to 30°C; after the stirring reaction is completed, the filtrate is evaporated to remove the solvent, and then 10 to 12 times of dichloromethane is added to dissolve the remaining substance, and then saturated sodium bicarbonate solution and deionized water are used for washing 2 to 3 times respectively, the organic phase is separated and dried with anhydrous potassium carbonate for 24 to 28 hours, the solvent in the organic phase is evaporated to remove, and ether with a mass of 4 to 5 times of the mass of the remaining organic phase is used for precipitation, and finally the filtered product is filtered and vacuum dried to constant weight to obtain the pretreated polyethylene glycol monomethyl ether.

[0013] As an optimization, the Mn of the polyethylene glycol monomethyl ether is 2000.

[0014] As an optimization, the modified methacrylate is prepared according to the following method: tetramethyl piperidinol is added to triethylamine at a mass ratio of 1:0.4-0.6, and stirred evenly to prepare a tetramethyl piperidinol solution; under the condition of a temperature of 0-5°C, acryloyl chloride is added to tetrahydrofuran at a mass ratio of 1.4-1.6:20-22, stirred evenly, and the tetramethyl piperidinol solution is uniformly added dropwise within 1-1.5 hours, and after the addition is completed, the reaction is stirred for 4-6 hours and then allowed to stand and filtered, the filtered product is added to a 50% ethanol aqueous solution with a mass fraction of 20-25 times the mass of the filtered product, and then filtered after recrystallization, and the filtered product is placed in a vacuum oven and dried to constant weight to obtain the modified methacrylate.

[0015] As an optimization, the co-embedded polymer is prepared by co-embedding pretreated polyethylene glycol monomethyl ether, polyvinyl pyridine and modified polymethyl methacrylate.

[0016] As an optimization, the pretreated polyethylene glycol monomethyl ether is prepared by grafting modification with 2-bromoisobutyryl bromide.

[0017] A microencapsulated gardenia yellow pigment is prepared by any of the above preparation methods.

[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0019] The present application uses a co-embedded polymer as a microcapsule wall material to microencapsulate Gardenia Yellow. Since Gardenia Yellow has good light resistance and heat resistance under neutral or alkaline conditions, but poor heat resistance and light resistance and is prone to browning at low pH values, the present application uses a co-embedded polymer to construct a pH-responsive microcapsule to avoid excessive release under acidic conditions, so that the release rate is slowed down or stopped under acidic conditions, but the release rate is accelerated under alkaline conditions. Therefore, the present application uses polyvinyl pyridine as a release switch. Polyvinyl pyridine is a weakly alkaline polymer that is ionized at medium and low pH values ​​and protonated at high pH values, thereby swelling, expanding the gap between its molecules, and then accelerating the release rate;

[0020] Polyethylene glycol monomethyl ether is used as the hydrophilic segment, which can quickly connect with gardenia yellow pigment in the oil phase and the hydrophilic segments gather inward to build an inner hydrophilic layer during the formation of microcapsules, thereby improving the overall stability.

[0021] In the present application, methyl methacrylate is modified with hindered amines, so that it has good UV resistance, improves the service life of the entire substrate, and prevents the substrate from yellowing and discoloring. In addition, since hindered amines have large steric hindrance, during the formation of microcapsules, the co-embedded polymer can force the other end to quickly build a complete microcapsule morphology inward through the intermolecular force between the side chains at one end facing outward. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are provided in detail. The raw materials used in the experimental part of the following examples are as follows:

[0024] Table 1 - Raw materials used in the experimental part

[0025]

[0026]

[0027] Example 1

[0028] S1. Add triethylamine to tetrahydrofuran at a mass ratio of 1:80, stir evenly to prepare a triethylamine solution for use; add 2-bromoisobutyryl bromide to tetrahydrofuran at a mass ratio of 1:120, stir evenly to prepare a 2-bromoisobutyryl bromide solution for use; at a temperature of 0-5°C, add polyethylene glycol monomethyl ether to toluene at a mass ratio of 1:3.5, wherein the polyethylene glycol monomethyl ether Mn is 2000, stir evenly, add triethylamine solution 3.5 times the mass of polyethylene glycol monomethyl ether, mix evenly, and uniformly add polyethylene glycol monomethyl ether dropwise within 2 hours. After the addition of 2-bromoisobutyryl bromide solution with a mass of 1.1 times that of methyl ether is completed, the reaction is stirred at a temperature of 25°C for 36 hours; after the stirring reaction is completed, the filtrate is evaporated to remove the solvent, and then 10 times the amount of dichloromethane is added to dissolve the remaining substance, and then washed twice with a saturated sodium bicarbonate solution and deionized water respectively, the organic phase is separated and dried with anhydrous potassium carbonate for 24 hours, the solvent in the organic phase is evaporated to remove the solvent, and 4 times the mass of ether is used for precipitation, and finally the filtered product is filtered and vacuum dried to constant weight to obtain pretreated polyethylene glycol monomethyl ether;

[0029] S2. Add tetramethylpiperidinol to triethylamine at a mass ratio of 1:0.4, stir evenly, and prepare a tetramethylpiperidinol solution; at a temperature of 0°C, add acryloyl chloride to tetrahydrofuran at a mass ratio of 1.4:20, stir evenly, and drop the tetramethylpiperidinol solution at a uniform rate within 1 hour. After the dropwise addition is completed, stir the reaction for 4 hours and then let it stand for filtration. Add the filtered product to a 50% ethanol aqueous solution with a mass fraction of 20 times the mass of the filtered product, recrystallize it, and filter it. Put the filtered product into a vacuum oven and dry it to constant weight to obtain modified methacrylate

[0030] S3. Under nitrogen protection, add pretreated polyethylene glycol monomethyl ether, vinyl pyridine, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:3.8:0.08:0.06:5.5, stir evenly, freeze and vacuumize with liquid nitrogen, fill with nitrogen to thaw 2 to 3 times, stir at 25°C for 25 minutes, heat to 55°C and react for 8 hours after stirring, add tetrahydrofuran 3 times the mass of pretreated polyethylene glycol monomethyl ether after the reaction is completed, stir evenly and dilute to stop the reaction, remove copper ions with an alumina chromatography column, and concentrate the solution after passing through the chromatography column with rotary evaporation. After rotary evaporation and concentration, add n-hexane 3 times the mass of the remaining solution and let it settle, filter after settling, and vacuum dry the filtered product to obtain a preliminary co-embedded product;

[0031] S4. Under nitrogen protection, add the preliminary co-embedded product, modified methyl methacrylate, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:24:1.8:0.15:7.5, stir evenly, freeze and evacuate with liquid nitrogen, fill with nitrogen to thaw twice, stir at 25°C for 25 minutes, heat to 55°C and react for 8 hours after stirring, add tetrahydrofuran 3 to 4 times the mass of the preliminary co-embedded product after the reaction is completed, stir evenly to dilute and stop the reaction, use an aluminum peroxide chromatography column to remove the copper ions therein, and concentrate the solution after passing through the chromatography column by rotary evaporation. After rotary evaporation and concentration, add 3 to 5 times the mass of the remaining solution of n-hexane and let it settle, filter after settling, and vacuum dry the filtered product to obtain a co-embedded polymer;

[0032] S5. Add the co-embedded polymer to dichloromethane at a mass ratio of 1:50, stir to dissolve, then add 0.6 times the mass of gardenia yellow pigment of the co-embedded polymer, and ultrasonically disperse for 20 minutes to obtain an oil phase; add the oil phase to a 0.4% polyvinyl alcohol aqueous solution at a volume ratio of 1:1 at 25°C, stir for 3 minutes at a speed of 1800 rpm, and then stir for 4 hours at a speed of 600 rpm, let stand to evaporate and remove the organic solvent, then perform ultrafiltration and centrifugation, and wash the centrifuged product with deionized water for 2 to 3 times, and freeze-dry to obtain microencapsulated gardenia yellow pigment.

[0033] Example 2

[0034] S1. Add triethylamine to tetrahydrofuran at a mass ratio of 1:85, stir evenly to prepare a triethylamine solution for use; add 2-bromoisobutyryl bromide to tetrahydrofuran at a mass ratio of 1:125, stir evenly to prepare a 2-bromoisobutyryl bromide solution for use; at a temperature of 3°C, add polyethylene glycol monomethyl ether to toluene at a mass ratio of 1:3.6, wherein the polyethylene glycol monomethyl ether Mn is 2000, stir evenly, add triethylamine solution 3.6 times the mass of polyethylene glycol monomethyl ether, mix evenly, and uniformly add polyethylene glycol monomethyl ether dropwise within 2.2 hours. After the addition of 2-bromoisobutyryl bromide solution with a mass of 1.2 times the mass of ether is completed, the reaction is stirred at a temperature of 28°C for 40 hours; after the stirring reaction is completed, the filtrate is evaporated to remove the solvent, and then 11 times the mass of dichloromethane is added to dissolve the remaining substance, and then washed twice with a saturated sodium bicarbonate solution and deionized water respectively, the organic phase is separated and dried with anhydrous potassium carbonate for 26 hours, the solvent in the organic phase is evaporated to remove the solvent, and 4.5 times the mass of ether is used for precipitation, and finally the filtered product is filtered and vacuum dried to constant weight to obtain pretreated polyethylene glycol monomethyl ether;

[0035] S2. Add tetramethylpiperidinol to triethylamine at a mass ratio of 1:0.5, stir evenly, and prepare a tetramethylpiperidinol solution; at a temperature of 3°C, add acryloyl chloride to tetrahydrofuran at a mass ratio of 1.5:21, stir evenly, and uniformly add the tetramethylpiperidinol solution dropwise within 1.2 hours. After the addition is completed, stir the reaction for 5 hours and then let it stand for filtration. Add the filtered product to a 50% ethanol aqueous solution with a mass fraction of 22 times the mass of the filtered product, recrystallize it, and filter it. Put the filtered product into a vacuum oven and dry it to constant weight to obtain modified methacrylate

[0036] S3. Under nitrogen protection, add pretreated polyethylene glycol monomethyl ether, vinyl pyridine, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:3.9:0.085:0.07:5.8, stir evenly, freeze and vacuumize with liquid nitrogen, fill with nitrogen and thaw twice, stir at 28°C for 30 minutes, heat to 60°C and react for 10 hours after stirring, add tetrahydrofuran 3.5 times the mass of pretreated polyethylene glycol monomethyl ether after stirring, dilute to stop the reaction, remove copper ions with an alumina chromatography column, and concentrate the solution after passing through the chromatography column with rotary evaporation. After rotary evaporation and concentration, add n-hexane 4 times the mass of the remaining solution and let it settle, filter after settling, and vacuum dry the filtered product to obtain a preliminary co-embedded product;

[0037] S4. Under nitrogen protection, add the preliminary co-embedded product, modified methyl methacrylate, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:25:2:0.17:7.:8, stir evenly, freeze and evacuate with liquid nitrogen, fill with nitrogen and thaw twice, stir at 28°C for 30 minutes, heat to 60°C and react for 10 hours after stirring, add tetrahydrofuran 3.5 times the mass of the preliminary co-embedded product after the reaction is completed, stir evenly and dilute to stop the reaction, remove the copper ions by aluminum peroxide chromatography column, and concentrate the solution after passing through the chromatography column by rotary evaporation. After rotary evaporation and concentration, add 3.5 times the mass of n-hexane of the remaining solution and let it settle, filter after settling, and vacuum dry the filtered product to obtain a co-embedded polymer;

[0038] S5. Add the co-embedded polymer to dichloromethane at a mass ratio of 1:55, stir to dissolve, then add 0.7 times the mass of gardenia yellow pigment of the co-embedded polymer, and ultrasonically disperse for 22 minutes to obtain an oil phase; at a temperature of 28°C, add the oil phase to a 0.4% polyvinyl alcohol aqueous solution at a volume ratio of 1:1, stir for 4 minutes at a speed of 1800 rpm, and then stir for 5 hours at a speed of 600 rpm, let stand to evaporate and remove the organic solvent, then perform ultrafiltration and centrifugation, and wash the centrifuged product twice with deionized water, and freeze-dry to obtain microencapsulated gardenia yellow pigment.

[0039] Example 3

[0040] S1. Add triethylamine to tetrahydrofuran at a mass ratio of 1:90, stir evenly to prepare a triethylamine solution for use; add 2-bromoisobutyryl bromide to tetrahydrofuran at a mass ratio of 1:130, stir evenly to prepare a 2-bromoisobutyryl bromide solution for use; at a temperature of 5°C, add polyethylene glycol monomethyl ether to toluene at a mass ratio of 1:3.8, wherein the polyethylene glycol monomethyl ether Mn is 2000, stir evenly, add triethylamine solution 3.7 times the mass of polyethylene glycol monomethyl ether, mix evenly, and uniformly add polyethylene glycol monomethyl ether dropwise within 2.5 hours. After the addition of 2-bromoisobutyryl bromide solution with a mass of 1.3 times that of methyl ether is completed, the reaction is stirred at a temperature of 30°C for 48 hours; after the stirring reaction is completed, the filtrate is evaporated to remove the solvent, and then 12 times the amount of dichloromethane is added to dissolve the remaining substance, and then saturated sodium bicarbonate solution and deionized water are used to wash 3 times respectively, the organic phase is separated and dried with anhydrous potassium carbonate for 28 hours, the solvent in the organic phase is evaporated to remove the solvent, and 5 times the mass of ether in the remaining organic phase is used for precipitation, and finally the filtered product is vacuum dried to constant weight to obtain pretreated polyethylene glycol monomethyl ether;

[0041] S2. Add tetramethylpiperidinol to triethylamine at a mass ratio of 1:0.6, stir evenly, and prepare a tetramethylpiperidinol solution; at a temperature of 5°C, add acryloyl chloride to tetrahydrofuran at a mass ratio of 1.6:22, stir evenly, and uniformly add the tetramethylpiperidinol solution dropwise within 1.5 hours. After the addition is completed, stir the reaction for 6 hours and then let it stand for filtration. Add the filtered product to a 50% ethanol aqueous solution with a mass fraction of 25 times the mass of the filtered product, recrystallize it, and filter it. Put the filtered product into a vacuum oven and dry it to constant weight to obtain modified methacrylate

[0042] S3. Under nitrogen protection, add pretreated polyethylene glycol monomethyl ether, vinyl pyridine, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:4.1:0.09:0.08:6, stir evenly, freeze and vacuumize with liquid nitrogen, fill with nitrogen to thaw 3 times, stir at 30°C for 35 minutes, heat to 65°C and react for 12 hours after stirring, add tetrahydrofuran 4 times the mass of pretreated polyethylene glycol monomethyl ether after the reaction is completed, stir evenly and dilute to stop the reaction, remove copper ions with an alumina chromatography column, and concentrate the solution after passing through the chromatography column with rotary evaporation. After rotary evaporation and concentration, add n-hexane 5 times the mass of the remaining solution and let it settle, filter after settling, and vacuum dry the filtered product to obtain a preliminary co-embedded product;

[0043] S4. Under nitrogen protection, add the preliminary co-embedded product, modified methyl methacrylate, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:26:2.2:0.18:8, stir evenly, freeze and evacuate with liquid nitrogen, fill with nitrogen to thaw 3 times, stir at 30°C for 35 minutes, heat to 65°C and react for 12 hours after stirring, add tetrahydrofuran 4 times the mass of the preliminary co-embedded product after the reaction is completed, stir evenly and dilute to stop the reaction, remove the copper ions by aluminum peroxide chromatography column, and concentrate the solution after passing through the chromatography column by rotary evaporation. After rotary evaporation and concentration, add n-hexane 5 times the mass of the remaining solution and let it settle, filter after settling, and vacuum dry the filtered product to obtain a co-embedded polymer;

[0044] S5. Add the co-embedded polymer to dichloromethane at a mass ratio of 1:60, stir to dissolve, then add 0.8 times the mass of gardenia yellow pigment of the co-embedded polymer, and ultrasonically disperse for 25 minutes to obtain an oil phase; at a temperature of 30°C, add the oil phase to a 0.4% polyvinyl alcohol aqueous solution at a volume ratio of 1:1, stir for 5 minutes at a speed of 1800 rpm, and then stir for 6 hours at a speed of 600 rpm, let stand to evaporate and remove the organic solvent, then perform ultrafiltration and centrifugation, and wash the centrifuged product with deionized water for 3 times, and freeze-dry to obtain microencapsulated gardenia yellow pigment.

[0045] Example 4

[0046] The only difference from Example 2 is step S5: replacing the "co-embedded polymer" with "preliminary co-embedded product".

[0047] Example 5

[0048] The only difference from Example 2 is that in step S5, the "co-embedded polymer" is replaced by "polyvinylpyridine".

[0049] Example 6

[0050] The only difference from Example 2 is that in step S4, "modified methyl methacrylate" is replaced by "methyl methacrylate".

[0051] Test Example 1

[0052] pH responsive release test of microcapsules:

[0053] The microcapsules prepared in Examples 1 to 6 were weighed in equal weight and placed in pH = 11 (sodium carbonate-sodium bicarbonate buffer), pH = 12 (sodium hydroxide), pH = 2 (hydrochloric acid), and pH = 3 (citric acid-disodium hydrogen phosphate buffer). After standing for 2 hours, the microcapsules were removed and the color change of the solution was observed;

[0054] Table 2 pH responsive release test results of microcapsules

[0055]

[0056] From the comparison of the experimental data of Examples 1 to 3 in Table 2, it can be found that the microcapsules prepared by the present invention exhibit good release function under alkaline conditions, and the release rate is slow under acidic conditions. This is because the co-embedded polymer used in the present application is pH responsive. When the pH of the solution increases, the polyvinyl pyridine segment can be protonated, changing its hydrophobicity to hydrophilicity, and the structure of the microcapsule changes, and the encapsulated repair agent is released.

[0057] In Examples 4 and 5, since only the preliminary co-embedded polymer was used in Example 4, the intermolecular force of the external chain segment forcing it to squeeze inward was lacking during the formation of the microcapsules, resulting in the easy formation of a vesicle structure, which led to a decrease in its loading capacity, or an incomplete closure phenomenon occurred during the formation of the microcapsules, resulting in a decrease in its pH response ability; in Example 5, since only polyvinylpyridine was used as the wall material, it lacked a hydrophilic chain segment and could not be linked to the gardenia yellow pigment in the oil phase, resulting in an extremely low loading rate of the finally generated microcapsules;

[0058] In Example 6, since unmodified methyl methacrylate was used as the outer chain segment, the shorter hydrophobic chain segments during the construction of the microcapsules also led to the same phenomenon as in Example 4, resulting in a decrease in the final loading rate.

[0059] Test Example 2

[0060] Anti-aging performance test of microcapsules:

[0061] The microcapsules were placed in pH = 11 (sodium carbonate-sodium bicarbonate buffer), pH = 12 (sodium hydroxide), pH = 2 (hydrochloric acid), and pH = 3 (citric acid-disodium hydrogen phosphate buffer), and the release rate of the microcapsules was measured after standing for 2 hours;

[0062] The microcapsules were placed in a xenon lamp weathering test chamber with a set temperature of 40°C, a humidity of 38%, and an irradiation intensity of 230 W / m 2 , irradiated with simulated natural light for 480 hours at a distance of 26 cm to accelerate aging; after aging, placed again in pH = 11 (sodium carbonate-sodium bicarbonate buffer), pH = 12 (sodium hydroxide) and pH = 2 (hydrochloric acid), pH = 3 (citric acid-disodium hydrogen phosphate buffer), and after standing for 2 hours, measured the microcapsule release rate and calculated the performance retention rate;

[0063] Performance retention rate = microcapsule release rate before aging / microcapsule release rate after aging

[0064] Table 3 Surface microstructure defect test results

[0065]

[0066] The anti-aging experiment is only conducted on Examples 1 to 3 and Example 6 mainly because it can be seen from the previous experiment that if Examples 4 and 5 are subjected to aging tests, since they do not have perfect microcapsule properties, the test results before and after will be slightly different or very different, making the test results meaningless;

[0067] In Table 3, it can be seen that Examples 1 to 3 have good anti-aging properties and good performance retention rates, but the results in Example 6 are not good. This is mainly because unmodified methyl methacrylate is used in Example 6, and its anti-aging properties, especially anti-ultraviolet performance, are greatly reduced, resulting in poor final test results.

[0068] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing microencapsulated gardenia yellow pigment, characterized in that: The microencapsulated gardenia yellow pigment is prepared by the following steps: S1. Under nitrogen protection, add pretreated polyethylene glycol monomethyl ether, vinyl pyridine, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:3.8-4.1:0.08-0.09:0.06-0.08, stir evenly, freeze and vacuumize with liquid nitrogen, fill with nitrogen to thaw 2-3 times, stir at 25-30°C for 25-35min, heat to 55-65°C after stirring for 8-12h, add tetrahydrofuran 3-4 times the mass of pretreated polyethylene glycol monomethyl ether after the reaction is completed, stir evenly and dilute to stop the reaction, remove copper ions from an alumina chromatography column, and concentrate the solution after passing through the chromatography column by rotary evaporation. After rotary evaporation and concentration, add 3-5 times the mass of n-hexane of the remaining solution and let it settle, filter after settling, and vacuum dry the filtered product to obtain a preliminary co-embedded product; S2. Under nitrogen protection, add the preliminary co-embedded product, modified methyl methacrylate, dibenzoyl peroxide and cuprous bromide to methanol in a mass ratio of 1:24-26:1.8-2.2:0.15-0.18, stir evenly, freeze and evacuate with liquid nitrogen, fill with nitrogen to thaw 2-3 times, stir at 25-30°C for 25-35min, heat to 55-65°C after stirring for 8-12h, add tetrahydrofuran 3-4 times the mass of the preliminary co-embedded product after the reaction is completed, stir evenly to dilute and stop the reaction, remove the copper ions by an alumina chromatography column, and concentrate the solution after passing through the chromatography column by rotary evaporation. After rotary evaporation and concentration, add 3-5 times the mass of n-hexane of the remaining solution and let it settle, filter after settling, and vacuum dry the filtered product to obtain a co-embedded polymer; S3. Add the co-embedded polymer to dichloromethane at a mass ratio of 1:50-60, stir to dissolve, then add 0.6-0.8 times the mass of the co-embedded polymer, and ultrasonically disperse for 20-25 minutes to obtain an oil phase; add the oil phase to the aqueous phase at a volume ratio of 1:1 at a temperature of 25-30°C, stir for 3-5 minutes at a speed of 1800 rpm, and then stir for 4-6 hours at a speed of 600 rpm, let stand to evaporate and remove the organic solvent, then perform ultrafiltration and centrifugation, and wash the centrifuged product with deionized water for 2-3 times, and freeze-dry to obtain microencapsulated gardenia yellow pigment.

2. The method for preparing microencapsulated gardenia yellow pigment according to claim 1, characterized in that: The water phase in S3 is a polyvinyl alcohol aqueous solution with a mass fraction of 0.4%.

3. The method for preparing microencapsulated gardenia yellow pigment according to claim 1, characterized in that: The pretreated polyethylene glycol monomethyl ether in S1 is prepared according to the following method: triethylamine is added to tetrahydrofuran at a mass ratio of 1:80-90, and the mixture is stirred evenly to prepare a triethylamine solution for use; 2-bromoisobutyryl bromide is added to tetrahydrofuran at a mass ratio of 1:120-130, and the mixture is stirred evenly to prepare a 2-bromoisobutyryl bromide solution for use; at a temperature of 0-5°C, polyethylene glycol monomethyl ether is added to toluene at a mass ratio of 1:3.5-3.8, the mixture is stirred evenly, and a triethylamine solution of 3.5-3.7 times the mass of polyethylene glycol monomethyl ether is added, and after mixing evenly, polyethylene glycol monomethyl ether is added dropwise at a uniform speed within 2-2.5 hours. After the addition of 2-bromoisobutyryl bromide solution with a mass of 1.1 to 1.3 times that of the monomethyl alcohol ether is completed, the reaction is stirred for 36 to 48 hours at a temperature of 25 to 30°C; after the stirring reaction is completed, the filtrate is evaporated to remove the solvent, and then 10 to 12 times of dichloromethane is added to dissolve the remaining substance, and then saturated sodium bicarbonate solution and deionized water are used for washing 2 to 3 times respectively, the organic phase is separated and dried with anhydrous potassium carbonate for 24 to 28 hours, the solvent in the organic phase is evaporated to remove the solvent, and ether with a mass of 4 to 5 times that of the remaining organic phase is used for precipitation, and finally the filtered product is filtered and vacuum dried to constant weight to obtain the pretreated polyethylene glycol monomethyl ether.

4. The method for preparing microencapsulated gardenia yellow pigment according to claim 3, characterized in that: The polyethylene glycol monomethyl ether Mn is 2000.

5. The method for preparing microencapsulated gardenia yellow pigment according to claim 1, characterized in that: The modified methacrylate is prepared according to the following method: tetramethyl piperidinol is added to triethylamine at a mass ratio of 1:0.4-0.6, and the mixture is stirred evenly to prepare a tetramethyl piperidinol solution; acryloyl chloride is added to tetrahydrofuran at a mass ratio of 1.4-1.6:20-22 at a temperature of 0-5°C, the mixture is stirred evenly, and the tetramethyl piperidinol solution is uniformly added dropwise within 1-1.5 hours, and after the addition is completed, the mixture is stirred for reaction for 4-6 hours, and then the mixture is allowed to stand for filtration, and the filtered product is added to an ethanol aqueous solution with a mass fraction of 50% and a mass fraction of 20-25 times the mass of the filtered product, and then the filtered product is recrystallized and filtered, and the filtered product is placed in a vacuum oven and dried to constant weight to obtain the modified methacrylate.

6. The method for preparing microencapsulated gardenia yellow pigment according to claim 1, characterized in that: The co-embedded polymer is prepared by co-embedding pretreated polyethylene glycol monomethyl ether, polyvinyl pyridine and modified polymethyl methacrylate.

7. The method for preparing microencapsulated gardenia yellow pigment according to claim 1, characterized in that: The pretreated polyethylene glycol monomethyl ether is prepared by grafting modification with 2-bromoisobutyryl bromide.

8. A microencapsulated gardenia yellow pigment, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 7.