Nano TiOx / Al2O3 high-energy wave-absorbing coating containing oxygen vacancies and preparation method of nano TiOx / Al2O3 high-energy wave-absorbing coating

By introducing oxygen vacancy into the Ti2AlC/Al2O3 or Ti3AlC2/Al2O3 composite coating, the nano-TiOx/Al2O3 high-energy absorbing coating is prepared by using a high-temperature oxidation treatment process, which solves the problem of narrow absorption bandwidth of the existing coating and achieves high-efficiency absorption The wave performance and high temperature oxidation resistance extend the coating life.

CN118978818AInactive Publication Date: 2024-11-19BEIJING JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411277951.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118978818A_ABST
    Figure CN118978818A_ABST
Patent Text Reader

Abstract

The invention discloses a nano TiOx / Al2O3 high-energy wave-absorbing coating containing oxygen vacancies and a preparation method of the nano TiOx / Al2O3 high-energy wave-absorbing coating. The coating comprises Al2O3 and nano TiOx containing the oxygen vacancies. The preparation method comprises the following steps: treating 80-95 wt% of Al2O3 powder and 5-20 wt% of Ti2AlC or Ti3AlC2 powder in mechanical powder mixing equipment until the powder is fully mixed, so as to obtain composite raw material powder; spraying the composite raw material powder on a nickel-based alloy matrix or a carbon fiber matrix by adopting a laser spraying process to obtain a basic coating; the basic coating is placed in a muffle furnace to be subjected to high-temperature oxidation treatment, the oxidation temperature ranges from 500 DEG C to 2000 DEG C, the oxidation time ranges from 0.1 h to 10 h, furnace cooling is conducted, and finally the nano TiOx / Al2O3 high-energy wave-absorbing coating containing the oxygen vacancies is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention relates to the field of material technology, and in particular to a nano-TiO x / Al2O3 high energy absorbing coating and preparation method thereof. Background technology:

[0002] As the world situation becomes increasingly unstable and complex, hypersonic aircraft such as stealth fighters, stealth ships and stealth missiles have also been vigorously developed in various countries, which can greatly reduce the radar reflection cross-section and improve the survival rate of equipment. In addition, due to friction with the air, the surface of hypersonic aircraft can reach 700℃ or even higher, which puts forward a strong demand for aircraft surface coatings with excellent radar stealth performance in high temperature environments. At present, the introduction of dielectric absorbers such as TiB2, TiC and TiO2 into the Al2O3 matrix to prepare absorbing coatings with excellent thermal stability and controllable dielectric loss has become a research hotspot. However, the single absorbing mechanism of dielectric loss absorbing coatings leads to a narrow effective absorbing bandwidth (EAB), which seriously limits the practical application of such coatings.

[0003] Existing studies have shown that introducing various defects such as oxygen and cation vacancy defects into absorbing materials through high-temperature heat treatment can effectively promote the dipole polarization relaxation loss of absorbing materials, thereby improving the absorbing performance. x ) is usually studied in oxygen-containing absorbing materials due to its low formation energy. For example, Fu et al. introduced oxygen vacancy defects into Ti2O3 without absorbing ability by carbothermal reduction and found that its EAB was enhanced from 2 GHz to 3.2 GHz. Although existing studies have confirmed that TiO x The excellent wave absorbing performance of the coating has been demonstrated, but the relevant coating products have not yet been manufactured and are still far from practical industrial applications.

[0004] At present, the use of high temperature resistant and highly conductive ternary MAX phase ceramics as dielectric absorbers has received widespread attention. Among them, Ti2AlC and Ti3AlC2 are typical representatives of MAX phases. During the oxidation process in an atmospheric environment above 800°C, Al diffuses outward from the A layer in Ti2AlC and Ti3AlC2 to form an Al2O3 layer and a non-stoichiometric TiC x After a long period of oxidation, Ti2AlC and Ti3AlC2 are oxidized to TiO containing oxygen vacancies. xand Al2O3. The outward diffusion of Al element can promote the excellent interface bonding between Ti2AlC and Ti3AlC2 and other metals or ceramics. These advantages show that Ti2AlC and Ti3AlC2 are ideal materials for manufacturing Al2O3-based dielectric lossy absorbing coatings on metal substrates. However, there is no research on introducing oxygen vacancy defects into Ti2AlC / Al2O3 and Ti3AlC2 / Al2O3 composite absorbing coatings to further improve the absorbing performance.

[0005] Based on the above discussion, oxygen vacancies were introduced into the Ti2AlC / Al2O3 or Ti3AlC2 / Al2O3 composite coatings by high temperature heat treatment to prepare nano-TiO2 with excellent performance. x / Al2O3 high energy absorbing coating is feasible. Summary of the invention:

[0006] The present invention is based on the fact that Ti2AlC and Ti3AlC2 can be decomposed and oxidized in high temperature air to form TiO containing oxygen vacancies. x Based on the characteristics of Al2O3, a high-temperature oxidation treatment process was creatively proposed to introduce oxygen vacancies into the composite coating prepared with Al2O3 powder and Ti2AlC or Ti3AlC2 powder as raw materials, and a nano-TiO2 with oxygen vacancies and controllable performance was successfully developed, which has excellent microwave absorption performance, high-temperature oxidation resistance, good interface bonding with the metal matrix, and reusability. x / Al2O3 high energy absorbing coating and preparation method thereof.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] The present invention provides a nano-TiO containing oxygen vacancies x / Al2O3 high energy absorbing coating, the coating comprises the following components by mass percentage: 80% to 95% Al2O3, 5% to 20% TiO x Wherein, the nano-TiO containing oxygen vacancies x The value of X is 0.5 to 1.9. The coating is prepared by laser spraying and subsequent high-temperature oxidation treatment; wherein the temperature and time of the high-temperature oxidation treatment can be artificially controlled, thereby achieving an effect in which the microwave absorption performance of the coating can be adjusted.

[0009] A further improvement of the present invention is that according to the GJB 2038A-2011 standard, for the coating sample with a size of 180 mm × 180 mm × 0.5-5 mm, under the test conditions of the radar absorbing material RAM reflectivity bow method in the frequency range of 2 GHz to 18 GHz, the effective absorbing bandwidth EAB (reflection loss RL <-10 dB) of the coating is greater than 10 GHz, and the minimum reflection loss RLmin Less than -20dB.

[0010] A further improvement of the present invention is that: the present invention provides a nano-TiO containing oxygen vacancies x / Al2O3 high energy absorbing coating, the coating has good interface bonding with the metal substrate, and the coating will not fall off, peel off, or delaminate after being subjected to high temperature thermal shock.

[0011] A further improvement of the present invention is that: the present invention provides a nano-TiO containing oxygen vacancies x / Al2O3 high-energy absorbing coating, the dense oxide layer on the surface of the coating can prevent oxygen atoms from entering the interior of the coating, thereby preventing it from further oxidation after long-term service in a high-temperature atmospheric environment, thereby achieving the effect of sustainable absorption and recycling, and extending the service life of the coating.

[0012] A further improvement of the present invention is that: the present invention provides a nano-TiO containing oxygen vacancies x / Al2O3 high-energy absorbing coating, the absorbing performance of the coating can be effectively regulated by artificially controlling the temperature and time of high-temperature oxidation treatment to meet usage requirements.

[0013] The present invention also provides the above-mentioned nano-TiO containing oxygen vacancies x A method for preparing a high-energy wave-absorbing coating of Al2O3 / Al2O3 includes the following steps: placing 80-95wt.% Al2O3 powder and 5-20wt.% Ti2AlC or Ti3AlC2 powder in a mechanical powder mixing device for 2-12 hours to fully mix to obtain a composite raw material powder; sandblasting pretreatment and preheating the surface of a nickel-based alloy substrate or a carbon fiber substrate, selecting a suitable laser spraying trajectory and process parameters to prepare a coating on the substrate surface to obtain a basic coating; the laser spraying parameters include: The optical power is 2500-3000W, the laser spot diameter is 2-2.5mm, the powder feeding amount is 5-7g / min, the scanning speed is 9-15m / min, the overlap rate is 70-85%, the defocus amount is +1-+3mm, the protective gas flow rate is 10-15L / min, and the powder feeding gas flow rate is 7-12L / min; the base coating is placed in a muffle furnace for high-temperature oxidation treatment, the oxidation temperature is 500°C-2000°C, the oxidation time is 0.1-10 hours, and the base coating is cooled with the furnace to finally obtain the nano-TiO containing oxygen vacancies. x / Al2O3 high energy absorbing coating.

[0014] Compared with the current prior art, the present invention has the following characteristics:

[0015] The present invention creatively proposes to introduce oxygen vacancies into the composite coating prepared with Al2O3 powder and Ti2AlC or Ti3AlC2 powder as raw materials by regulating the high temperature oxidation treatment process, and successfully develops a nano-TiO2 with oxygen vacancies that has excellent microwave absorption performance, high temperature oxidation resistance, good interface bonding with the metal matrix, and reusability. x / Al2O3 high-energy absorbing coating and its preparation method. The dense oxide layer on the surface of the coating can prevent oxygen atoms from entering the interior of the coating, thereby preventing it from further oxidation after long-term service in a high-temperature atmospheric environment, thereby achieving the effect of sustainable absorption and recycling, and extending the service life of the coating; the inner layer of the coating has a good interface with the metal substrate; in addition, the absorbing performance of the coating can be effectively regulated by artificially controlling the temperature and time of the high-temperature oxidation treatment to meet the use requirements. The high-temperature oxidation treatment process described in the present invention is simple, easy to operate, and low in cost, and is suitable for large-scale industrial production. Description of the drawings:

[0016] Figure 1 A nano-TiO containing oxygen vacancies according to Example 1 of the present invention x / Scanning electron microscope image of Al2O3 high energy absorbing coating;

[0017] Figure 2 A nano-TiO containing oxygen vacancies according to Example 1 of the present invention x / Comparison of measured reflection loss RL values ​​of Al2O3 high energy absorbing coating before and after oxidation;

[0018] Figure 3 A nano-TiO containing oxygen vacancies according to Example 1 of the present invention x / XRD comparison diagram of Al2O3 high energy absorbing coating before and after oxidation;

[0019] Figure 4 A nano-TiO containing oxygen vacancies according to Example 1 of the present invention x / XPS graph of Al2O3 high energy absorbing coating; Specific implementation method:

[0020] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The elements and features described in one embodiment of the present invention may be combined with the elements and features shown in one or more other embodiments. It should be noted that for the purpose of clarity, the representation and description of components and processes that are not related to the present invention and are known to those of ordinary skill in the art are omitted in the description. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.

[0021] In order to meet the urgent military demand for hypersonic aircraft to continue to have radar stealth and wave absorbing performance after the friction with the atmosphere generates high temperature, the inventor creatively proposed to regulate the high temperature oxidation treatment process to introduce oxygen vacancies in the composite coating prepared with Al2O3 powder and Ti2AlC or Ti3AlC2 powder as raw materials, and successfully developed a nano-TiO2 with oxygen vacancies that has excellent wave absorbing performance, high temperature oxidation resistance, good interface bonding with the metal matrix, and reusability. x / Al2O3 high-energy absorbing coating and its preparation method. The dense oxide layer on the surface of the coating can prevent oxygen atoms from entering the interior of the coating, thereby preventing it from further oxidation after long-term service in a high-temperature atmospheric environment, thereby achieving the effect of sustainable absorption and recycling, and extending the service life of the coating; the absorbing performance of the coating can be effectively regulated by artificially controlling the temperature and time of high-temperature oxidation treatment to meet the use requirements.

[0022] The present invention also provides the above-mentioned nano-TiO containing oxygen vacancies x A method for preparing a / Al2O3 high energy absorbing coating, the preparation method comprising the following steps:

[0023] S1. Place 80-95wt.% Al2O3 powder and 5-20wt.% Ti2AlC or Ti3AlC2 powder in a mechanical powder mixing device for 2-12 hours until they are fully mixed to obtain a composite raw material powder;

[0024] S2. Pre-treat and preheat the surface of the nickel-based alloy substrate or the carbon fiber substrate by sandblasting, select appropriate laser spraying trajectory and process parameters to prepare a coating on the substrate surface to obtain a basic coating; the laser spraying parameters include: laser power 2500-3000W, laser spot diameter 2-2.5mm, powder feeding amount 5-7g / min, scanning speed 9-15m / min, overlap rate 70-85%, defocusing amount +1-+3mm, protective gas flow rate 10-15L / min, powder feeding gas flow rate 7-12L / min;

[0025] S3, placing the base coating in a muffle furnace for high temperature oxidation treatment, the oxidation temperature is 500°C to 2000°C, the oxidation time is 0.1 to 10 hours, and cooling with the furnace, finally obtaining the nano-TiO containing oxygen vacancies x / Al2O3 high energy absorbing coating.

[0026] The present invention is described in detail below in conjunction with specific implementation modes.

[0027] Example 1

[0028] Example 1 provides a nano-TiO containing oxygen vacancies x / Al2O3 high energy absorbing coating and preparation method thereof, the preparation method comprising:

[0029] 85wt.% Al2O3 powder and 15wt.% Ti2AlC powder are placed in a mechanical powder mixing device for 2 hours to be fully mixed to obtain a composite raw material powder, and the composite raw material powder is sprayed on a nickel-based alloy substrate by a laser spraying device to obtain a base coating with a size of 180mm×180mm×1.1mm; then, the base coating is placed in a muffle furnace for high-temperature oxidation treatment at an oxidation temperature of 950°C for an oxidation time of 2 hours, and then cooled with the furnace to obtain the nano-TiO2 containing oxygen vacancies. x / Al2O3 high energy absorbing coating. Figure 1 As shown in (a), the coating surface is filled with dense Ti oxide. Figure 1 As shown in (b), diffusely distributed nanoscale TiO x Grains. Figure 2 As shown in the figure, the base coating before oxidation does not achieve effective wave absorption, and the nano-TiO containing oxygen vacancies obtained after oxidation x The effective absorbing bandwidth (reflection loss RL<-10dB) of the / Al2O3 high energy absorbing coating is up to 11.2GHz, including the entire X and Ku bands. min The signal increased from -3.77dB before oxidation to -26.91dB after oxidation. Figure 3 and Figure 4 As shown in Figure 2, the coating consists of Al2O3 and TiO containing oxygen vacancies. x The composition of the composite is quartz crystal, in which oxygen vacancies account for 60.98%, and the calculated value of x is 0.78.

[0030] Example 2

[0031] Example 2 provides a nano-TiO containing oxygen vacancies x / Al2O3 high energy absorbing coating and preparation method thereof, the preparation method comprising:

[0032] 85wt.% Al2O3 powder and 15wt.% Ti3AlC2 powder are placed in a mechanical powder mixing device for 2 hours to be fully mixed to obtain a composite raw material powder, and the composite raw material powder is sprayed on a nickel-based alloy substrate by a laser spraying device to obtain a base coating with a size of 180mm×180mm×1.1mm; then, the base coating is placed in a muffle furnace for high-temperature oxidation treatment at an oxidation temperature of 950°C for an oxidation time of 2 hours, and then cooled with the furnace to obtain the nano-TiO2 containing oxygen vacancies. x / Al2O3 high energy absorbing coating.

[0033] Example 3

[0034] Example 3 provides a nano-TiO containing oxygen vacancies x / Al2O3 high energy absorbing coating and preparation method thereof, the preparation method comprising:

[0035] 85wt.% Al2O3 powder and 15wt.% Ti2AlC powder are placed in a mechanical powder mixing device for 2 hours to be fully mixed to obtain a composite raw material powder, and the composite raw material powder is sprayed on a nickel-based alloy substrate by a laser spraying device to obtain a base coating with a size of 180mm×180mm×1.1mm; then, the base coating is placed in a muffle furnace for high-temperature oxidation treatment at an oxidation temperature of 950°C for 10 hours, and then cooled with the furnace to obtain the nano-TiO containing oxygen vacancies. x / Al2O3 high energy absorbing coating.

[0036] The present invention creatively proposes to introduce oxygen vacancies into the composite coating prepared with Al2O3 powder and Ti2AlC or Ti3AlC2 powder as raw materials by regulating the high temperature oxidation treatment process, and successfully develops a nano-TiO2 with oxygen vacancies that has excellent microwave absorption performance, high temperature oxidation resistance, good interface bonding with the metal matrix, and reusability. x / Al2O3 high-energy absorbing coating and its preparation method. The dense oxide layer on the surface of the coating can prevent oxygen atoms from entering the interior of the coating, thereby preventing it from further oxidation after long-term service in a high-temperature atmospheric environment, thereby achieving the effect of sustainable absorption and recycling, and extending the service life of the coating; the inner layer of the coating has a good interface with the metal substrate; in addition, the absorbing performance of the coating can be effectively regulated by artificially controlling the temperature and time of the high-temperature oxidation treatment to meet the use requirements. The high-temperature oxidation treatment process described in the present invention is simple, easy to operate, and low in cost, and is suitable for large-scale industrial production.

[0037] Finally, it should be noted that: although the present invention and its advantages have been described in detail above, it should be understood that various changes, substitutions and transformations can be made without exceeding the spirit and scope of the present invention as defined by the appended claims. Moreover, the scope of the present invention is not limited to the specific embodiments of the processes, devices, means, methods and steps described in the specification. It will be easily understood by those of ordinary skill in the art from the disclosure of the present invention that existing and future processes, devices, means, methods or steps that perform substantially the same functions as the corresponding embodiments described herein or obtain substantially the same results as the corresponding embodiments described herein can be used according to the present invention. Therefore, the appended claims are intended to include such processes, devices, means, methods or steps within their scope.

Claims

1. A nano-TiO containing oxygen vacancies x / Al2O3 high energy absorbing coating and preparation method thereof, characterized in that: The coating comprises the following components by mass percentage: 80% to 95% Al2O3, 5% to 20% TiO x ; Wherein, the Al2O3 and TiO x The sum of the components is 100%.

2. A nano-TiO containing oxygen vacancies x / Al2O3 high energy absorbing coating and preparation method thereof, characterized in that: Nano-TiO with oxygen vacancies x The X value in is 0.5 to 1.

9.

3. Nano-TiO containing oxygen vacancies according to claim 1 x / Al2O3 high energy absorbing coating, characterized in that: According to the GJB 2038A-2011 standard, for the coating sample with a size of 180mm×180mm×0.5~5mm, under the test conditions of the radar absorbing material RAM reflectivity bow method in the frequency range of 2GHz~18GHz, the effective absorbing bandwidth EAB (reflection loss RL<-10dB) of the coating is greater than 10GHz, and the minimum reflection loss RL min Less than -20dB.

4. A nano-TiO containing oxygen vacancies as claimed in claim 1 x / Al2O3 high energy absorbing coating preparation method, characterized in that, The method comprises the following steps: Step 1, placing 80-95wt.% Al2O3 powder and 5-20wt.% Ti2AlC or Ti3AlC2 powder in a mechanical powder mixing device for 2-12 hours until fully mixed to obtain a composite raw material powder; Step 2, pre-treating and preheating the surface of the nickel-based alloy substrate or the carbon fiber substrate by sandblasting, selecting appropriate laser spraying trajectory and process parameters to prepare a coating on the substrate surface to obtain a basic coating; the laser spraying parameters include: laser power 2500-3000W, laser spot diameter 2-2.5mm, powder feeding amount 5-7g / min, scanning speed 9-15m / min, overlap rate 70-85%, defocusing amount +1-+3mm, shielding gas flow rate 10-15L / min, powder feeding gas flow rate 7-12L / min; Step 3, placing the base coating in a muffle furnace for high temperature oxidation treatment, the oxidation temperature is 500°C to 2000°C, the oxidation time is 0.1 to 10 hours, and the furnace is cooled to finally obtain the nano-TiO containing oxygen vacancies. x / Al2O3 high energy absorbing coating.

Citation Information

Patent Citations

  • Al2O3 and Ti2AlC composite wave-absorbing coating and preparation method thereof

    CN116285468A

  • High-temperature oxidation resistant wave-absorbing ceramic coating with double-layer structure and preparation method of high-temperature oxidation resistant wave-absorbing ceramic coating