Phosphorus-nitrogen-containing aniline oligomer modified boron nitride fireproof anti-corrosion bifunctional coating composition and preparation method thereof

By using a dual-function coating composition with phosphorus-containing aniline oligomer modified boron nitride in steel structure coatings, the problems of cumbersome and poor compatibility of fire-resistant and anticorrosion coatings in the prior art are solved, and efficient fire protection is achieved Anti-corrosion and corrosion resistance limits improve the stability and environmental protection of the coating.

CN118978825AActive Publication Date: 2024-11-19XIAMEN UNIV

Patent Information

Application Number
CN202411119364.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-19
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Among the existing steel structure coatings, fire-resistant coatings and corrosion-resistant coatings usually have only a single function. The coatings with both fire-resistant and corrosion-resistant functions are cumbersome, cost-effective and poor compatibility, resulting in limited protection effects.

Method used

Using a phosphorus-containing aniline oligomer modified boron nitride fire-resistant and anti-corrosion dual-function coating composition, the aniline oligomer and boron nitride are dispersed in deionized water by ammonium dihydrogen phosphate, combining the expanded flame retardant system and functional assistance. The agent forms a coating that combines the modified boron nitride dispersion with the matrix resin and the curing agent to enhance compatibility and protection performance.

Benefits of technology

The integrated coating design is realized, the corrosion and fire resistance performance is improved, the service life of the coating is extended, the corrosion resistance and fire resistance limits are enhanced, and the environmental significance of the product is improved through the composite ternary expansion system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978825A_ABST
    Figure CN118978825A_ABST
Patent Text Reader

Abstract

The invention discloses a phosphorus-nitrogen-containing aniline oligomer modified boron nitride fireproof anti-corrosion dual-functional coating composition and a preparation method thereof. The coating composition is prepared from matrix resin, modified boron nitride dispersion liquid, an intumescent flame-retardant system, a functional additive and a curing agent. The modified boron nitride dispersion liquid comprises an ammonium dihydrogen phosphate-terminated aniline oligomer, boron nitride and a dispersion medium. According to the modified boron nitride composite coating with the fireproof and anti-corrosion functions, a corrosive medium is blocked through the labyrinth effect of the two-dimensional material boron nitride and the passivation and capture effects of the aniline oligomer and ammonium dihydrogen phosphate, so that efficient corrosion prevention is achieved; and fire prevention is realized through the action of catalyzing carbon formation by using non-combustible gas generated by burning the aniline oligomer and polyphosphoric acid generated by ammonium dihydrogen phosphate. According to the invention, the ammonium dihydrogen phosphate terminated aniline oligomer enhances the compatibility of boron nitride in matrix resin through pi-pi conjugation, can effectively improve the fire endurance and anticorrosion effect of the product, and further prolongs the service life of the organic coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fireproof and anticorrosion coatings, and specifically relates to a phosphorus-nitrogen-containing aniline oligomer-modified boron nitride fireproof and anticorrosion dual-function coating composition and a preparation method thereof. Background Art

[0002] The rapid development of industries such as marine transportation, marine engineering, new energy development, and new chemical materials has put forward higher requirements for coatings for offshore equipment such as offshore oil platforms and offshore steel structure buildings. These coatings are not only required to have excellent anti-corrosion properties, but also require good fire retardant properties. However, in existing steel structure coatings, fire retardant coatings and anti-corrosion coatings usually only have a single function. Although there are coatings on the market that have both fire retardant and anti-corrosion functions, the coating process is often cumbersome and costly, and due to poor compatibility, it may cause peeling, thereby affecting the protective effect. Therefore, the development of a dual-function fire retardant coating that has both anti-corrosion function and fire retardant performance, realizing the integrated design of anti-corrosion and protective coatings, can solve the problems of cumbersome processes caused by the mixed use of fire retardant coatings and anti-corrosion coatings.

[0003] As an emerging discipline that has just emerged and attracted much attention in the past decade, the application of nanomaterials in the field of coatings has become a hot topic of research. In particular, the application of nanotechnology to achieve halogen-free flame retardants and fillers is of great significance for the development of ultra-thin fire-resistant and anti-corrosion coatings for steel structures. Boron nitride nanosheets have shown important application prospects in fire prevention and corrosion prevention due to their unique two-dimensional structure. However, due to their high surface energy and large volume, boron nitride nanosheets are easy to agglomerate in the resin matrix, which limits their application in fire-resistant and anti-corrosion coatings. Summary of the invention

[0004] The present invention aims to overcome the defects of the prior art and provides a phosphorus-nitrogen-containing aniline oligomer-modified boron nitride fire-retardant and anti-corrosion dual-function coating composition.

[0005] Another object of the present invention is to provide a method for preparing the above-mentioned phosphorus-nitrogen-containing aniline oligomer-modified boron nitride fire-retardant and anti-corrosion dual-functional coating composition.

[0006] The technical solution of the present invention is as follows:

[0007] A phosphorus-nitrogen-containing aniline oligomer-modified boron nitride fireproof and anticorrosive dual-functional coating composition is prepared from a base resin, a modified boron nitride dispersion, an intumescent flame retardant system, a functional additive and a curing agent, wherein:

[0008] The structural formula of the modified boron nitride in the modified boron nitride dispersion is

[0009]

[0010] In a preferred embodiment of the present invention, the modified boron nitride dispersion is prepared by dispersing ammonium dihydrogen phosphate-capped aniline oligomers and boron nitride in deionized water; the ammonium dihydrogen phosphate-capped aniline oligomers are prepared by doping aniline oligomers with ammonium dihydrogen phosphate through protonation; and the aniline oligomers are prepared from aniline and p-phenylenediamine sulfate under acidic conditions.

[0011] Further preferably, the preparation method of the modified boron nitride dispersion comprises the following steps:

[0012] A. Dissolve aniline and p-phenylenediamine sulfate in dilute ammonium dihydrogen phosphate solution;

[0013] B. dissolving ammonium persulfate (APS) in a dilute ammonium dihydrogen phosphate solution, and then dropping the solution into the material obtained in step A at a speed of 2-4 s / drop, stirring while dropping; after the dropwise addition is completed, continuing to stir the reaction at the same speed for 0.8-1.2 h to obtain a precipitate, and subjecting the precipitate to solid-liquid separation and drying to obtain the ammonium dihydrogen phosphate-terminated aniline oligomer;

[0014] C. Boron nitride and the above ammonium dihydrogen phosphate-terminated aniline oligomer are ultrasonically dispersed in a dispersion medium for 2-4 hours respectively, and then the two are mixed and stirred at room temperature for 4-8 hours to fully react to obtain a modified boron nitride dispersion.

[0015] More preferably, in the dilute ammonium dihydrogen phosphate solution, the ratio of ammonium dihydrogen phosphate to deionized water is 1.1-1.2 g:230-260 mL, and the mass ratio of the boron nitride to the ammonium dihydrogen phosphate-terminated aniline oligomer is 1:1-3.

[0016] More preferably, the stirring speed in step C is 400-600 r / min.

[0017] In a preferred embodiment of the present invention, the base resin is selected from water-based epoxy resin, silicone resin, acrylic resin, polyurethane resin, polyester resin, alkyd resin; the curing agent is selected from diaminodiphenylmethane, polyamide, diaminodiphenyl sulfone, meta-phenylenediamine, meta-phenylenediamine and polyetheramine.

[0018] Further preferably, in the intumescent flame retardant system, APP:MEL:PER=2:1:1 (APP is ammonium polyphosphate, MEL is melamine, and PER is pentaerythritol).

[0019] Further preferably, the functional additives include a leveling agent, a defoaming agent, a dispersant and an anti-settling agent.

[0020] The preparation method of the phosphorus-nitrogen-containing aniline oligomer-modified boron nitride fire-retardant and anti-corrosion dual-functional coating composition comprises the following steps:

[0021] (1) stirring and dispersing the base resin, modified boron nitride dispersion, intumescent flame retardant system and functional additive for 1-2 hours;

[0022] (2) Add the curing agent to the material obtained in step (1) and stir and disperse for 1-2 hours to obtain the product.

[0023] In a preferred embodiment of the present invention, the stirring speeds in steps (1) and (2) are both 1500-2000 r / min.

[0024] The beneficial effects of the present invention are:

[0025] 1. The phosphoric acid-terminated aniline oligomer of the present invention has the functions of passivating the metal surface, "capturing" iron ions, and promoting the formation of complexes and other corrosion inhibition effects; and the nitrogen content in the aniline oligomer is also very high, and a large amount of non-combustible gases such as NO and NO2 will be generated during the combustion process, which dilutes the oxygen concentration and plays a gas phase flame retardant role.

[0026] 2. The ammonium dihydrogen phosphate in the present invention will eventually produce polyphosphoric acid during the combustion process to catalyze carbonization, thereby achieving excellent flame retardant properties.

[0027] 3. The boron nitride two-dimensional material in the present invention forms a maze effect by virtue of its large specific surface area, effectively preventing the diffusion of corrosion factors, and has stable chemical properties and high temperature resistance. When burned, it can form the skeleton of the protective system of the residual carbon layer, effectively preventing the coating from cracking under flames, and improving the corrosion resistance and fire resistance of the product.

[0028] 4. The ammonium dihydrogen phosphate-terminated aniline oligomer-modified boron nitride in the present invention is modified by π-π conjugated non-covalent bonds to obtain N, P-modified boron nitride nanosheets, which greatly enhances the compatibility of the boron nitride inorganic material in the organic resin, thereby effectively extending the service life of the coating.

[0029] 5. The present invention develops a composite ternary expansion system, which comprehensively applies flame retardant-smoke suppression synergistic flame retardant technology and halogen-free flame retardant technology containing phosphorus, nitrogen, boron nitride, inorganic flame retardants, etc., to improve the fire resistance limit of the product and further give the product environmental significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of the preparation process of ammonium dihydrogen phosphate-terminated aniline oligomer (AT-P) and modified boron nitride (BN-AT-P) in Examples 1 to 4 of the present invention.

[0031] Figure 2 IR spectra of aniline oligomer (AT), ammonium dihydrogen phosphate-terminated aniline oligomer (AT-P) and modified boron nitride (BN-AT-P) in Examples 1 to 4 of the present invention.

[0032] Figure 3 It is a comparison chart of the change of the back surface temperature of the coated steel plate with time in Comparative Example 1 and Examples 1 to 4 of the present invention.

[0033] Figure 4 It is the macroscopic morphology of the matrix resin expanded carbon layer in Comparative Example 1 and Examples 1 to 4 of the present invention. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0035] Comparative Example 1

[0036] (1) 100 parts by weight of an aqueous epoxy resin, 80 parts by weight of an intumescent flame retardant system (APP:MEL:PER=2:1:1), 0.24 parts by weight of a BYK-066N defoamer, 0.24 parts by weight of a BYK-P104 dispersant, and 0.24 parts by weight of a BYK-410 anti-settling agent are placed in a coating tank and uniformly dispersed by oscillation in a high-speed disperser.

[0037] (2) Add 100 parts by weight of a polyamide curing agent to step (1), and disperse the mixture evenly by oscillation in a high-speed disperser to obtain a coating material APP / MEL / PER.

[0038] (3) The material obtained in step (2) is coated on a steel plate using a wire rod coater to prepare a coating sample. The steel plate used to test the anti-corrosion performance is coated with a thickness of about 60 μm, and the steel plate used to test the fire resistance performance is coated with a thickness of about 1 mm.

[0039] (4) The material obtained in step (2) was poured into a preheated specific mold to prepare flame retardant test specimens, which were cured at room temperature for 24 h, 70° C. for 2 h, and 120° C. for 4 h.

[0040] (5) After curing, the samples prepared in steps (3) and (4) were subjected to performance tests. The relevant test results are shown in Tables 1 and Figure 3 , Figure 4 shown.

[0041] Example 1

[0042] (1) Weigh 1.15 g of ammonium dihydrogen phosphate and dilute it with deionized water to obtain 250 mL of dilute ammonium dihydrogen phosphate solution. Measure 150 mL of dilute ammonium dihydrogen phosphate solution into a 250 mL round-bottom flask. Weigh 2.956 g of p-phenylenediamine sulfate and add it to the flask for ultrasonic dispersion. After the p-phenylenediamine sulfate is completely dissolved, weigh 1.853 g of aniline and add it to the flask. At the same time, weigh 4.541 g of ammonium persulfate (APS) and dissolve it with 50 mL of dilute ammonium dihydrogen phosphate solution and add it to a constant pressure dropping funnel. Put the flask into a low-temperature circulation tank at -5°C, and control the constant pressure dropping funnel to slowly drip into the flask at a speed of 3s / drop, stirring while dripping. After the dripping is completed, continue to stir and react for 1 hour. After the reaction is completed, filter the product by suction, and then wash it with deionized water until the filtrate is neutral to obtain a filter cake. The filter cake was placed in a vacuum oven and dried at 60°C for 24 h. The obtained product was ball milled using a planetary ball mill to obtain an infrared spectrum as shown in FIG. Figure 2 The ammonium dihydrogen phosphate-terminated aniline oligomer (AT-P) shown;

[0043] (2) Weigh 100 mg of boron nitride and 200 mg of ammonium dihydrogen phosphate-terminated aniline oligomer and add them to 25 mL of deionized water. Ultrasonicate for 1 hour to obtain a modified boron nitride dispersion. (The preparation principles of the above steps (1) and (2) are as follows Figure 1 As shown, the infrared spectrum of the modified boron nitride is as follows Figure 2 (shown)

[0044] (3) 100 parts by weight of waterborne epoxy resin, 0.5 parts by weight of the above-mentioned ammonium dihydrogen phosphate-terminated aniline oligomer modified boron nitride, 80 parts by weight of an intumescent flame retardant system (APP:MEL:PER=2:1:1), 0.24 parts by weight of a BYK-066N defoamer, 0.24 parts by weight of a BYK-P104 dispersant, and 0.24 parts by weight of a BYK-410 anti-settling agent are placed in a coating tank and dispersed uniformly by oscillation in a high-speed disperser.

[0045] (4) Add 100 parts by weight of a polyamide curing agent to the material obtained in step (3), and disperse the mixture evenly by oscillation in a high-speed disperser to obtain a coating material APP / MEL / PER-0.5% BAP.

[0046] (5) The material obtained in step (4) is coated on a steel plate using a wire rod coater to prepare a coating sample. The steel plate used to test the anti-corrosion performance is coated with a thickness of about 60 μm, and the steel plate used to test the fire retardancy is coated with a thickness of about 1 mm.

[0047] (6) The material obtained in step (4) was poured into a preheated specific mold to prepare flame retardant test specimens, which were cured at room temperature for 24 h, 70° C. for 2 h, and 120° C. for 4 h.

[0048] (7) After curing, the samples prepared in steps (5) and (6) were subjected to performance tests. The relevant test results are shown in Tables 1 and Figure 3 , Figure 4 shown.

[0049] Example 2

[0050] Step (1) and step (2) are the same as in Example 1.

[0051] (3) 100 parts by weight of waterborne epoxy resin, 1 part by weight of the above-mentioned ammonium dihydrogen phosphate-terminated aniline oligomer modified boron nitride, 80 parts by weight of an intumescent flame retardant system (APP:MEL:PER=2:1:1), 0.24 parts by weight of a BYK-333 leveling agent, 0.24 parts by weight of a BYK-066N defoamer, 0.24 parts by weight of a BYK-P104 dispersant, and 0.24 parts by weight of a BYK-410 anti-settling agent are placed in a coating tank and uniformly dispersed by oscillation with a high-speed disperser.

[0052] (4) Add 100 parts by weight of a polyamide curing agent to the material obtained in step (3), and disperse the mixture evenly by oscillation in a high-speed disperser to obtain a coating material APP / MEL / PER-1% BAP.

[0053] Steps (5) to (7) are the same as in Example 1.

[0054] The relevant test results are shown in Table 1 and Figure 3 , Figure 4 shown.

[0055] Example 3

[0056] Step (1) and step (2) are the same as in Example 1.

[0057] (3) 100 parts by weight of waterborne epoxy resin, 1.5 parts by weight of the above-mentioned ammonium dihydrogen phosphate-terminated aniline oligomer modified boron nitride, 80 parts by weight of an intumescent flame retardant system (APP:MEL:PER=2:1:1), 0.24 parts by weight of a BYK-066N defoamer, 0.24 parts by weight of a BYK-P104 dispersant, and 0.24 parts by weight of a BYK-410 anti-settling agent are placed in a coating tank and dispersed uniformly by oscillation in a high-speed disperser.

[0058] (4) Add 100 parts by weight of a polyamide curing agent to the material obtained in step (3), and disperse the mixture evenly by oscillation in a high-speed disperser to obtain a coating material APP / MEL / PER-1.5% BAP.

[0059] Steps (5) to (7) are the same as in Example 1.

[0060] The relevant test results are shown in Table 1 and Figure 3, Figure 4 shown.

[0061] Example 4

[0062] Step (1) and step (2) are the same as in Example 1.

[0063] (3) 100 parts by weight of waterborne epoxy resin, 2 parts by weight of the above-mentioned ammonium dihydrogen phosphate-terminated aniline oligomer modified boron nitride, 80 parts by weight of an intumescent flame retardant system (APP:MEL:PER=2:1:1), 0.24 parts by weight of a BYK-066N defoamer, 0.24 parts by weight of a BYK-P104 dispersant, and 0.24 parts by weight of a BYK-410 anti-settling agent are placed in a coating tank and dispersed uniformly by oscillation in a high-speed disperser.

[0064] (4) Add 100 parts by weight of a polyamide curing agent to the material obtained in step (3), and disperse the mixture evenly by oscillation in a high-speed disperser to obtain a coating material APP / MEL / PER-2% BAP.

[0065] Steps (5) to (7) are the same as in Example 1.

[0066] The relevant test results are shown in Table 1 and Figure 3 , Figure 4 shown.

[0067] Table 1 Fire and corrosion resistance properties of ammonium dihydrogen phosphate-terminated aniline oligomer-modified boron nitride coating

[0068]

[0069] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A phosphorus-nitrogen-containing aniline oligomer-modified boron nitride fire-retardant and anti-corrosion dual-functional coating composition, Features: It is prepared from base resin, modified boron nitride dispersion, expansion flame retardant system, functional additives and curing agent, wherein: The structural formula of the modified boron nitride in the modified boron nitride dispersion is 2. A fireproof and anticorrosive dual-function coating composition containing phosphorus and nitrogen aniline oligomer modified boron nitride as claimed in claim 1, Features: The modified boron nitride dispersion is prepared by dispersing ammonium dihydrogen phosphate-terminated aniline oligomer and boron nitride in deionized water; the ammonium dihydrogen phosphate-terminated aniline oligomer is prepared by doping aniline oligomer with ammonium dihydrogen phosphate through protonation; and the aniline oligomer is prepared by aniline and p-phenylenediamine sulfate under acidic conditions.

3. A fireproof and anticorrosive dual-function coating composition containing phosphorus and nitrogen aniline oligomer modified boron nitride as claimed in claim 2, Features: The preparation method of the modified boron nitride dispersion comprises the following steps: A. Dissolve aniline and p-phenylenediamine sulfate in dilute ammonium dihydrogen phosphate solution; B. dissolving ammonium persulfate in a dilute ammonium dihydrogen phosphate solution, and then dropping the solution into the material obtained in step A at a rate of 2-4 s / drop, stirring while dropping; after the dropwise addition is completed, continuing to stir the reaction at the same rate for 0.8-1.2 h to obtain a precipitate, and subjecting the precipitate to solid-liquid separation and drying to obtain the ammonium dihydrogen phosphate-terminated aniline oligomer; C. Boron nitride and the above ammonium dihydrogen phosphate-terminated aniline oligomer are ultrasonically dispersed in a dispersion medium for 2-4 hours respectively, and then the two are mixed and stirred at room temperature for 4-8 hours to fully react to obtain a modified boron nitride dispersion.

4. A fireproof and anticorrosive dual-function coating composition containing phosphorus and nitrogen aniline oligomer modified boron nitride as claimed in claim 3, Features: In the dilute ammonium dihydrogen phosphate solution, the ratio of ammonium dihydrogen phosphate to deionized water is 1.1-1.2 g:230-260 mL, and the mass ratio of the boron nitride to the ammonium dihydrogen phosphate-terminated aniline oligomer is 1:1-3.

5. A fireproof and anticorrosive dual-function coating composition containing phosphorus and nitrogen aniline oligomer modified boron nitride as claimed in claim 3, Features: The stirring speed in step C is 400-600 r / min.

6. A fire-retardant and anti-corrosion dual-functional coating composition of boron nitride modified by phosphorus-nitrogen aniline oligomer according to any one of claims 1 to 5, Features: The matrix resin is selected from waterborne epoxy resin, silicone resin, acrylic resin, polyurethane resin, polyester resin, and alkyd resin; the curing agent is selected from diaminodiphenylmethane, polyamide, diaminodiphenyl sulfone, metaphenylenediamine, metaphenylenediamine, and polyetheramine.

7. A fireproof and anticorrosive dual-function coating composition containing phosphorus and nitrogen aniline oligomer modified boron nitride as claimed in claim 6, Features: In the intumescent flame retardant system, APP:MEL:PER=2:1:

1.

8. A fireproof and anticorrosive dual-function coating composition containing phosphorus and nitrogen aniline oligomer modified boron nitride as claimed in claim 6, Features: The functional additives include leveling agents, defoaming agents, dispersants and anti-settling agents.

9. A method for preparing a fire-retardant and anti-corrosion dual-functional coating composition containing phosphorus and nitrogen aniline oligomer modified boron nitride according to any one of claims 1 to 8, Features: The steps include: (1) stirring and dispersing the base resin, modified boron nitride dispersion, intumescent flame retardant system and functional additive for 1-2 hours; (2) Add the curing agent to the material obtained in step (1) and stir and disperse for 1-2 hours to obtain the product.

10. The preparation method according to claim 9, Features: The stirring speed in steps (1) and (2) is 1500-2000 r / min.

Citation Information

Patent Citations

  • Doped-state polyaniline epoxy paint and preparation method thereof

    CN103980798A

  • Hexagonal boron nitride epoxy anticorrosive wear-resistant paint as well as preparation method and application thereof

    CN106752676A

  • Boron nitride dispersant based on aniline oligomer derivative and application of boron nitride dispersant

    CN107365261A

  • Inorganic phosphoric acid doped polyaniline multifunctional coating and preparation method thereof

    CN108948841A

  • Composite material, water-based anticorrosive wear-resistant coating and preparation method and application thereof

    CN112812297A

Cited By

  • Hexagonal boron nitride-guanazole-sodium hexametaphosphate flame-retardant resin coating and preparation method thereof

    CN119552551A