Composite perfluorooctylsulfonamide multifunctional additive and preparation method thereof

By mixing perfluorooctylsulfonamide with sodium butylsulfonate in a specific proportion and preparing a composite additive, the problem of insufficient stability and foam inhibition and defoaming performance in coatings is solved, and the problem of significantly improving the The stability and wetting and dispersing properties of the coating are effectively avoided pinholes and intra-film bubbles.

CN118978826AInactive Publication Date: 2024-11-19YANGZHOU POLYTECHNIC INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411056907.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When perfluorohexylsulfonamide is used in coatings, the stability, compatibility and foam-repressing and defoaming properties of the coating are insufficient, and there are problems such as pinholes and intra-film foaming.

Method used

Using a composite perfluorooctylsulfonamide multifunctional additive, the compounding and suction filtration are carried out by mixing perfluorooctylsulfonamide with sodium butylsulfonate in a specific proportion, and after reflux reaction and distillation of solvents, the solvent is prepared. The obtained composite additive is added to the coating formula to improve the stability of the coating and foam-resisting and defoaming performance.

Benefits of technology

It significantly reduces the surface tension of the coating film, improves the stability and compatibility of the coating, effectively solves problems such as pinholes and film bubbles, and enhances the stability of wetting and dispersion and foam suppression and defoaming performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978826A_ABST
    Figure CN118978826A_ABST
Patent Text Reader

Abstract

The invention discloses a composite perfluorooctylsulfonamide multifunctional auxiliary agent and a preparation method thereof. The composite perfluorooctylsulfonamide multifunctional auxiliary agent comprises perfluorooctylsulfonamide and sodium butyl sulfonate in a mass ratio of (7.8-8.3): 1. The preparation method of the composite perfluorooctylsulfonamide multifunctional auxiliary agent comprises the following steps: by taking perfluorooctylsulfonyl fluoride and isobutylamine as raw materials and cyclohexane as a solvent, carrying out reflux reaction, distilling to remove the solvent to obtain perfluorooctylsulfonamide, then adding sodium butanesulfonate, and by taking cyclohexane as a solvent, stirring, compounding and carrying out suction filtration to obtain the composite perfluorooctylsulfonamide multifunctional auxiliary agent. The composite perfluorooctylsulfonamide multifunctional additive can remarkably improve the stability, compatibility and foam inhibition and defoaming performance of a coating, reduce the surface tension of a coating film and effectively solve the problems of pinholes, bubbles in the film and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite perfluorooctane sulfonamide multifunctional auxiliary agent and a preparation method thereof. Background Art

[0002] Fluorocarbon surfactants have higher surface activity than ordinary hydrocarbon surfactants because of their fluorocarbon chains, which have both high oleophobicity and extreme hydrophobicity. They can be used in textile, leather, papermaking, coatings and other industries. Perfluorohexylsulfonamide, as a widely used multifunctional additive for coatings, can have a good wetting and dispersion effect on the pigments in the formula to prevent re-agglomeration, so that the paint layer can obtain excellent performance. Despite this, there are still prominent problems in the use of perfluorohexylsulfonamide, such as the stability, compatibility and anti-foaming and defoaming performance of the coating prepared by adding perfluorohexylsulfonamide to the coating, and there are problems such as pinholes and bubbles in the membrane. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a composite perfluoro multifunctional additive perfluorooctane sulfonamide, which can be added to the coating formula to significantly improve the stability, compatibility and anti-foaming and defoaming properties of the coating, reduce the surface tension of the coating, and effectively solve problems such as pinholes and bubbles in the film.

[0004] The composite perfluorooctane sulfonamide multifunctional additive of the present invention comprises perfluorooctane sulfonamide and sodium butyl sulfonate in a mass ratio of 7.8-8.3:1.

[0005] Preferably, the mass ratio of perfluorooctane sulfonamide to sodium butyl sulfonate is 8.05:1.

[0006] The present invention also provides a preparation method of the composite perfluorooctane sulfonamide multifunctional additive, which comprises taking perfluorooctane sulfonyl fluoride and isobutylamine as raw materials, taking cyclohexane as solvent, carrying out reflux reaction, distilling off the solvent, obtaining perfluorooctane sulfonamide, adding sodium butyl sulfonate for compounding, taking cyclohexane as solvent, stirring and filtering to obtain the composite perfluorooctane sulfonamide.

[0007] Preferably, the mass ratio of perfluorooctane sulfonyl fluoride:isobutylamine:sodium butyl sulfonate is 7.8-8.3:9.1-9.6:1.

[0008] Preferably, the reflux reaction temperature is 75°C-80°C, and the reflux reaction time is 4-5h.

[0009] The present invention also provides a composite emulsion, which comprises the composite perfluorooctane sulfonamide multifunctional additive, or comprises the composite perfluorooctane sulfonamide multifunctional additive prepared by the preparation method of the composite perfluorooctane sulfonamide multifunctional additive.

[0010] Beneficial effects: Compared with the coating additive perfluorohexyl sulfonamide used on the market, the composite perfluorooctane sulfonamide multifunctional additive of the present invention can significantly reduce the surface tension of the coating film after being added to the coating formula, improve the stability, compatibility and anti-foaming and defoaming properties of the coating, and can more effectively solve problems such as pinholes and bubbles in the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 The scanning electron microscope photos of the anti-corrosion coatings of Example 3 and Comparative Example 2;

[0012] Figure 2 is a graph of the contact angles of the anti-corrosion coatings of Example 3 and Comparative Example 2;

[0013] Figure 3 It is a graph of the antifoaming and defoaming performance in the composite emulsions of Example 2, Comparative Example 1, and Comparative Example 3. DETAILED DESCRIPTION

[0014] The technical solution of the present invention is described in detail below through embodiments, but the protection scope of the present invention is not limited to the embodiments.

[0015] Example 1

[0016] In a three-necked flask, 56.5 g of perfluorooctane sulfonyl fluoride (industrial grade, with a purity of 90%, Kanos, Hubei Wuhan Kanos Technology Co., Ltd.) and a small amount of cyclohexane solvent were added in sequence, the temperature was slowly raised to 78°C, and stirred for 20 min. In a separatory funnel, 90 ml of isobutylamine (analytical grade, Huifengda, Shandong Jinan Huifengda Chemical Co., Ltd.) was added dropwise three times every 30 min. After reflux reaction for 4.5 h, the solvent was distilled off to obtain perfluorooctane sulfonamide, and then 7 g of sodium butane sulfonate (industrial grade, kmk, Wuhan Kamik Technology Co., Ltd.) was added. Cyclohexane was used as solvent. The mixture was stirred, compounded, and filtered to obtain a composite perfluorooctane sulfonamide multifunctional additive.

[0017] Example 2

[0018] 9 g of epoxy resin (E-51, Changzhou Jushun Composite Materials Co., Ltd.), 13 g of polyurethane (single component, Qingdao Enze Chemical Co., Ltd.), 4.0 g of sodium hexadecylbenzenesulfonate (CAS No. 65143-89-7, Shandong Suihua Biotechnology Co., Ltd.), and 4.0 g of lauryl alcohol polyoxyethylene ether (LAEO-50, Hai'an Petrochemical Plant, Jiangsu Province) were added dropwise into 50 ml of anhydrous ethanol, and stirred evenly after mixing. The temperature was slowly raised to 40° C. After 30 minutes, 3.32 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in Example 1 was added, the temperature was raised to 55° C., and the reaction was kept warm for 4.5 hours. After cooling to room temperature, an epoxy-polyurethane composite emulsion was obtained, and the content of the composite perfluorooctane sulfonamide multifunctional additive was about 5.0%.

[0019] Example 3

[0020] Two coats of the composite emulsion prepared in Example 2 were sprayed on the treated tinplate, and one coat was sprayed again one day later. The coating was dried for 150 hours at a humidity of 60% and a temperature of 25°C to obtain an anti-corrosion coating with a total dry film thickness of 120 μm.

[0021] Example 4

[0022] In Example 2, the steps of “adding 3.32 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 after 30 min and heating to 55° C.” are changed to “adding 0.664 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 after 30 min and heating to 55° C.” are performed. Otherwise, a composite emulsion is obtained in the same manner as in Example 2, and the content of the composite perfluorooctane sulfonamide multifunctional additive is about 1.0%.

[0023] Example 5

[0024] In Example 2, the steps of “adding 3.32 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 after 30 min and heating to 55° C.” are changed to “adding 1.99 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 after 30 min and heating to 55° C.” are performed. Otherwise, a composite emulsion is prepared in the same manner as in Example 2, and the content of the composite perfluorooctane sulfonamide multifunctional additive is about 3.0%.

[0025] Example 6

[0026] In Example 2, the steps of “adding 3.32 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 after 30 min and heating to 55° C.” are changed to “adding 4.65 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 after 30 min and heating to 55° C.” are performed. Otherwise, a composite emulsion is obtained in the same manner as in Example 2, and the content of the composite perfluorooctane sulfonamide multifunctional additive is about 7.0%.

[0027] Example 7

[0028] In Example 2, the steps of “adding 3.32 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 after 30 min and heating to 55° C.” are changed to “adding 5.98 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 after 30 min and heating to 55° C.” are performed. Otherwise, a composite emulsion is prepared in the same manner as in Example 2, and the content of the composite perfluorooctane sulfonamide multifunctional additive is about 9.0%.

[0029] Comparative Example 1

[0030] In Example 2, the method of “adding 3.32 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 after 30 minutes and heating to 55° C.” is changed to “adding 3.28 g of perfluorohexyl sulfonamide additive after 30 minutes and heating to 55° C.” is carried out in the same manner as in Example 2. A composite emulsion is obtained, and the content of perfluorohexyl sulfonamide additive is about 5.0%.

[0031] Comparative Example 2

[0032] Two coats of the composite emulsion prepared in Comparative Example 1 were sprayed on the treated tinplate, and one coat was sprayed again one day later. The coating was dried for 150 hours at a humidity of 60% and a temperature of 25°C to obtain an anti-corrosion coating with a total dry film thickness of 120 μm.

[0033] Comparative Example 3

[0034] In Example 2, the content of “3.32 g of the composite perfluorooctane sulfonamide multifunctional additive prepared in the above Example 1 was added after 30 minutes, and the temperature was raised to 55°C” was changed to “30 minutes later, the temperature was raised to 55°C”. Otherwise, a composite emulsion was prepared in the same manner as in Example 2, and the content of the composite perfluorooctane sulfonamide multifunctional additive was 0.

[0035] Performance Testing

[0036] The anti-corrosion coatings of Example 3 and Comparative Example 2 were photographed using a scanning electron microscope (SEM), and the results were as follows: Figure 1 a. Figure 1 As shown in b, it can be seen that the anti-corrosion coating containing about 5.0% of the composite perfluorooctane sulfonamide multifunctional additive ( Figure 1 a) contains about 5.0% perfluorohexylsulfonamide additive coating ( Figure 1 b) Smoother, better compatibility, can effectively solve problems such as pinholes and bubbles in the membrane.

[0037] The contact angle test of the anti-corrosion coatings of Example 3 and Comparative Example 2 was performed using a HSD-GX521 series water drop angle tester (SGC-QH6, Dongguan Huishida Instruments). The results are as follows: Figure 2 a. Figure 2 b. The contact angle can be used to measure the wetting performance of the coating surface. The smaller the contact angle, the better the wetting performance of the liquid on the solid surface. Figure 2 a. Figure 2 bIt can be seen that Figure 2 The contact angle of a is 76.2°, Figure 2 The contact angle of b is 81.4°. By comparison, the contact angle of the anti-corrosion coating containing about 5.0% of the composite perfluorooctane sulfonamide multifunctional additive is ( Figure 2 a) The contact angle of the coating containing about 5.0% perfluorohexylsulfonamide additive ( Figure 2b) decreased by 5.2°. The above results show that the surface wetting performance of the anti-corrosion coating containing about 5.0% of the composite perfluorooctane sulfonamide multifunctional additive is enhanced, and it has excellent wetting and dispersion stability.

[0038] The composite emulsions of Examples 2, 4-7 and Comparative Example 3 were observed for appearance, calcium ion stability, storage stability and pencil hardness of the composite emulsions, and the results are shown in Table 1. The pencil hardness test of the paint film and the storage stability test of the composite emulsion were measured according to standards GB / T6739-2006 and GB6753.3-86, respectively. The calcium ion stability test was performed by adding 1% CaCl2 solution to the emulsion, stirring it evenly, and judging the calcium ion stability of the emulsion based on whether there was sedimentation and flocculation.

[0039] Table 1

[0040]

[0041] As can be seen from Table 1, the emulsion containing about 5.0% of the composite perfluorooctane sulfonamide additive has the best comprehensive performance in terms of calcium ion stability, storage stability and pencil hardness. It can be seen that the comprehensive performance of the composite emulsion is related to the amount of composite perfluorooctane sulfonamide additive added. Excessive or insufficient perfluorooctane sulfonamide has an adverse effect on the stability and pencil hardness of the composite emulsion, which may be related to the regularity of the molecular arrangement.

[0042] The composite emulsions of Example 2, Comparative Example 1 and Comparative Example 3 were tested for static surface tension using a German Kruss-K11 quality control surface tension meter. The results showed that the surface tension of the composite emulsion containing about 5.0% composite perfluorooctane sulfonamide additive in Example 2 was 16.8 mN / m, the surface tension of the composite emulsion containing about 5.0% perfluorohexane sulfonamide additive in Comparative Example 1 was 22.7 mN / m, and the surface tension of the emulsion without any additive in Comparative Example 3 was 30.1 mN / m. It can be seen that the composite emulsion containing about 5.0% composite perfluorooctane sulfonamide additive can significantly reduce the surface tension of the emulsion, so that the emulsion has stronger wetting performance, will not produce surface defects, has good foam control performance, and has excellent dispersion stability.

[0043] Under the same experimental conditions, the composite emulsion containing about 5.0% of the composite perfluorooctane sulfonamide multifunctional additive of Example 2, the composite emulsion containing about 5.0% of the perfluorohexyl sulfonamide additive of Comparative Example 1, and the composite emulsion without any additive of Comparative Example 3 were added to three measuring cylinders for comparative experiments. The results are as follows: Figure 3 a- Figure 3 c. Figure 3 a- Figure 3 c It can be seen that the composite emulsion of Comparative Example 3 generates the most bubbles ( Figure 3c), the composite emulsion of Comparative Example 1 produced fewer bubbles ( Figure 3 b), the composite emulsion of Example 2 produces the least bubbles ( Figure 3 a). This shows that the composite emulsion of Example 2 has less foaming, and the bubbles after foaming can be eliminated quickly, and the emulsion has better foaming and defoaming performance.

[0044] The composite perfluorooctane sulfonyl fluoride and isobutylamine are reacted and compounded with sodium butyl sulfonate to obtain a composite perfluorooctane sulfonamide additive, which is a multifunctional additive with excellent wetting and leveling properties and high-efficiency defoaming properties. In terms of wettability, leveling, anti-foaming and defoaming properties, anti-shrinkage compatibility, etc., it has more significant effects than the combined effects of general wetting agents and dispersants, and can effectively solve the problems of pinholes and bubbles in the coating film that are difficult to solve with other additives.

[0045] The above-mentioned technologies not specifically mentioned are all referred to the prior art.

[0046] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.

Claims

1. A composite perfluorooctane sulfonamide multifunctional additive, characterized in that: It contains perfluorooctane sulfonamide and sodium butyl sulfonate in a mass ratio of 7.8-8.3:

1.

2. The composite perfluorooctane sulfonamide multifunctional additive according to claim 1, characterized in that: The mass ratio of perfluorooctane sulfonamide to sodium butyl sulfonate is 8.05:

1.

3. The method for preparing the composite perfluorooctane sulfonamide multifunctional additive according to claim 1 or 2, characterized in that: Perfluorooctane sulfonyl fluoride and isobutylamine are used as raw materials and cyclohexane is used as solvent. After reflux reaction, the solvent is distilled off to obtain perfluorooctane sulfonamide, and then sodium butyl sulfonate is added for compounding, and cyclohexane is used as solvent, and the product is obtained by stirring and filtering.

4. The method for preparing the composite perfluorooctane sulfonamide multifunctional additive according to claim 3, characterized in that: The mass ratio of perfluorooctane sulfonyl fluoride: isobutylamine: sodium butyl sulfonate is 7.8-8.3:9.1-9.6:

1.

5. The method for preparing the composite perfluorooctane sulfonamide multifunctional additive according to claim 3, characterized in that: The reflux reaction temperature is 75°C-80°C, and the reflux reaction time is 4-5h.

6. A composite emulsion, characterized in that: The invention comprises the composite perfluorooctane sulfonamide multifunctional additive according to claim 1 or 2, or comprises the composite perfluorooctane sulfonamide multifunctional additive prepared by the preparation method of the composite perfluorooctane sulfonamide multifunctional additive according to any one of claims 3 to 5.