TPO (Thermoplastic Polyolefin) waterproof coiled material for metal film-coated plate and preparation method of TPO waterproof coiled material

By using a TPO waterproof coil composed of a polyolefin layer and an adhesive layer on the metal coating plate, combined with the hot press forming process, the problem of insufficient peel strength and durability of the waterproof coil in the prior art is solved, and a higher level of The boiling resistance and simplified production process reduce costs and environmental pollution.

CN118978869APending Publication Date: 2024-11-19SUZHOU FUNIKA MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411069176.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing waterproof coils of metal coated plates have insufficient peel strength, boiling resistance and durability during construction, and the production process is complex and the cost is high, and the solvent volatilization leads to pollution.

Method used

The TPO waterproof coil consisting of a polyolefin layer and an adhesive layer is used. The polyolefin layer is made of ethylene propylene copolymer, filler, antioxidant and light stabilizer. The adhesive layer is grafted with maleic anhydride polyolefin and maleic The acid anhydride grafted polypropylene wax, high molecular weight epoxy resin and hydrogenated petroleum resin are composed of acid anhydride grafting polypropylene wax, high molecular weight epoxy resin and hydrogenated petroleum resin. The metal coated plate is prepared by high-speed stirring and twin screw extrusion mechanism, and combined with hot pressing molding.

Benefits of technology

It improves the peel strength, boiling resistance and durability of metal coating plates, simplifies production processes, reduces costs and environmental pollution, and meets or exceeds industry standards in a comprehensive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980319400000051
    Figure BDA0004980319400000051
Patent Text Reader

Abstract

The invention provides a TPO (Thermoplastic Polyolefin) waterproof coiled material for a metal film-coated plate. The TPO waterproof coiled material consists of a polyolefin layer and a bonding layer, the polyolefin layer is prepared from the following raw materials in parts by weight: 50-90 parts of an ethylene-propylene copolymer, 12-30 parts of filler, 0.1-0.5 part of an antioxidant and 0.5-1 part of a light stabilizer; the bonding layer is prepared from the following raw materials in parts by weight: 60-90 parts of maleic anhydride grafted polyolefin, 3-8 parts of maleic anhydride grafted polypropylene wax, 10-20 parts of high molecular weight epoxy resin and 4-10 parts of hydrogenated petroleum resin. The invention also provides a preparation method of the TPO waterproof coiled material. The TPO waterproof coiled material provided by the invention can effectively improve the peel strength, boiling water boiling resistance and durability of a metal film-coated plate, so that the comprehensive performance of the metal film-coated plate can reach or exceed the requirements of the group standard T / CBMCA 017-2020 Coated Steel Plate for Building.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of waterproof coiled materials, and in particular relates to a TPO waterproof coiled material for metal coated plates and a preparation method thereof. Background Art

[0002] At present, the basic structure of the first-level waterproofing of industrial and commercial light steel roofs is: metal plate, vapor barrier, insulation layer, non-woven fabric, polymer waterproofing membrane (such as TPO). The wind-resistant performance of the roof system must be tested and specified in accordance with the specifications in the construction design. The material construction must be constructed in sequence according to the above-mentioned structural levels, and no structural material can be missing, and the total construction cost is high. Most of the existing steel structure roofs are designed for secondary waterproofing, relying only on vertical lock edge self-waterproofing, and no waterproof layer is set. Since the color steel plates on the roof are connected by rivets, and the rivets are exposed, the rivets will be corroded as the use time increases, resulting in a decrease in connection strength and a potential leakage risk on the roof. At present, there are two main maintenance options for light steel roofs: one is to directly replace the damaged color steel plates; the other is to polish and remove rust on the color steel plates, and use acrylic waterproof coating or chloroprene glue to bond TPO waterproof membranes for maintenance. The construction personnel cost of the above two options is high, and the material price is also high.

[0003] Exposed TPO waterproofing membranes have been proven to have an outdoor service life of more than 20 years at home and abroad. In recent years, exposed TPO waterproofing membranes have been compounded onto metal plates in factories using polymer adhesive films according to specific processes, which can greatly increase the corrosion resistance and aging resistance of metal plates, with a durability of more than 20 years; in addition, the weldability of TPO waterproofing membranes can ensure that the overlap of TPO waterproofing membranes has good waterproof sealing performance after welding.

[0004] The TPO metal-coated panels currently produced on the market are generally made of purchased polymer adhesive films and TPO coils. The polymer adhesive film layer and the TPO layer are first aligned and bonded with solvent-based glue, and then connected to a metal plate (such as galvanized steel plate) at high temperature. The production process is relatively complicated, and there is a lot of waste of glue and adhesive film. The volatilization of organic solvents will cause pollution and the cost is relatively high.

[0005] The patent with publication number CN118082315A discloses "laminated metal plate, preparation method and roof". The polymer adhesive layer described therein is divided into a first adhesive layer, a second adhesive layer and a third adhesive layer, which are prepared by processes such as casting, laminating and blowing. The adhesive layer and the polymer waterproof layer are then hot-pressed together, and then hot-pressed with the steel plate to obtain a metal laminated plate. This process is relatively complicated. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a TPO waterproof membrane for metal-clad panels, which can effectively improve the peel strength, boiling water resistance and durability of the metal-clad panels, so that the comprehensive performance of the metal-clad panels reaches or exceeds the requirements of the group standard T / CBMCA 017-2020 "Film-clad steel panels for construction".

[0007] In order to solve the above technical problems, the technical solution of the present invention is:

[0008] A TPO waterproofing coiled material for metal film-coated plates, comprising a polyolefin layer and an adhesive layer; the polyolefin layer is made of the following raw materials in parts by weight: 50-90 parts of ethylene-propylene copolymer, 12-30 parts of filler, 0.1-0.5 parts of antioxidant, and 0.5-1 parts of light stabilizer; the adhesive layer is made of the following raw materials in parts by weight: 60-90 parts of maleic anhydride grafted polyolefin, 3-8 parts of maleic anhydride grafted polypropylene wax, 10-20 parts of high molecular weight epoxy resin, and 4-10 parts of hydrogenated petroleum resin.

[0009] Furthermore, the thickness of the polyolefin layer of the present invention is 0.5-1.8 mm, and the thickness of the adhesive layer is 100-200 μm.

[0010] Furthermore, the melt flow rate of the ethylene-propylene copolymer of the present invention measured at 230° C. and 2.16 kg is 1-3 g / 10 min.

[0011] Furthermore, the filler of the present invention is composed of titanium dioxide and calcium carbonate in a weight ratio of 1:2.

[0012] Furthermore, the maleic anhydride grafted polyolefin of the present invention has a melt flow rate of 3-5 g / 10 min at 190° C. and 2.16 kg, and a maleic anhydride grafting rate of 1-5%. 1-5% of anhydride is grafted onto the polyolefin molecular chain, which does not affect its compatibility with the polyolefin and can produce an adhesive effect with the metal plate.

[0013] Furthermore, the maleic anhydride grafted polypropylene wax of the present invention has a softening point of 120-160°C and an average molecular weight of 5000-20000. Maleic anhydride grafted polypropylene wax introduces a strongly polar side group on the non-polar molecular main chain, which can serve as a bridge to enhance the adhesion and compatibility between polar materials and non-polar materials.

[0014] Furthermore, the epoxy equivalent of the high molecular weight epoxy resin of the present invention is 2800-3500, and the softening point is 135-155° C. The high molecular weight epoxy resin can greatly improve the adhesion between the TPO waterproofing membrane and the base metal plate.

[0015] Furthermore, the softening point of the hydrogenated petroleum resin of the present invention is 100-130° C. Adding hydrogenated petroleum resin into the system can make the adhesive layer instantly bond with the metal plate at high temperature.

[0016] Another technical problem to be solved by the present invention is to provide a method for preparing the TPO waterproof membrane for metal coated panels.

[0017] To solve the above technical problems, the technical solution is:

[0018] A method for preparing a TPO waterproofing membrane for a metal-coated plate comprises the following steps:

[0019] S1. The ethylene-propylene copolymer, filler, antioxidant, and light stabilizer were weighed and added to a high-speed mixer for dispersion for 30 min, and then transferred to a twin-screw extruder for granulation to obtain a polyolefin layer pellet for standby use;

[0020] S2. The maleic anhydride grafted polyolefin, maleic anhydride grafted polypropylene wax, high molecular weight epoxy resin, hydrogenated petroleum resin were weighed and added to a high-speed mixer for dispersion for 30 min, and then transferred to a twin-screw extruder for granulation to obtain a bonding layer of pellets for standby;

[0021] S3. The polyolefin layer pellets obtained in step S1 are conveyed to the feeding hopper of extruder 1 of the multi-layer sheet screw extruder, and the bonding layer pellets obtained in step S2 are conveyed to the feeding hopper of extruder 2 of the multi-layer sheet screw extruder, and the feeding is started after the temperature of extruder 1 and extruder 2 rises to the set temperature, and the composite sheet consisting of the polyolefin layer and the bonding layer is obtained by extrusion and calendaring;

[0022] S4. The composite sheet obtained in step S3 is cooled, trimmed, rolled and packaged to obtain a TPO waterproof membrane for metal-coated panels.

[0023] Furthermore, in step S1 of the present invention, the speed of the high-speed mixer is 400-500 r / min, the temperature of the feeding section of the twin-screw extruder is 200°C, the temperatures of the three sections at the center of the screw are 210°C, 215°C, and 205°C, the die temperature is 200°C, and the screw speed is 400 r / min;

[0024] In step S2, the speed of the high-speed mixer is 400-500 r / min, the temperature of the feeding section of the twin-screw extruder is 180°C, the temperatures of the three sections in the center of the screw are 190°C, 195°C, and 185°C, the die temperature is 180°C, and the screw speed is 200 r / min;

[0025] In the step S3, the temperature of the extruder 1 is set as follows: 110°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 208°C in zones 1-8, 210°C, 210°C, 210°C in zones 1-3, 210°C in melt pump zone, 207°C in zones 1-11 of the mold, 209°C in the left plate zone, and 209°C in the right plate zone; the temperature of the extruder 2 is set as follows: 100°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 188°C in zones 1-8, 185°C, 185°C, 185°C in zones 1-3, 185°C in melt pump zone, 187°C in zones 1-11 of the mold, 189°C in the left plate zone, and 189°C in the right plate zone; the main engine speed of the multilayer sheet screw extruder is 24r / min, and the feeding speed ratio is 1.

[0026] The method for preparing a metal film-faced plate by using the TPO waterproofing membrane for metal film-faced plate of the present invention comprises:

[0027] The TPO waterproofing coil and metal plate used for the metal film-coated plate are fed into the laminating machine in a stacking order, and the metal film-coated plate is obtained by instantaneous hot pressing. The metal plate is at least one of galvanized steel plate, aluminum-zinc steel plate, aluminum-magnesium-zinc steel plate, stainless steel plate, and aluminum alloy plate, and the thickness of the metal plate is 0.4-1.2 mm.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1) The present invention develops a TPO waterproofing membrane for metal-coated panels by adjusting the material formula and process, which can effectively solve the problems of alignment of the membrane and the film during the coating process, environmental protection treatment of solvent-based glue, and complex process. The TPO waterproofing membrane can be directly hot-pressed with a metal plate to produce a metal-coated panel. The physical and mechanical properties and durability of the metal-coated panel reach or exceed those of the conventional process-coated panel.

[0030] 2) The manufacturing process of the present invention is simple and energy-efficient, and has good economic, environmental and social benefits, and has broad application prospects. DETAILED DESCRIPTION

[0031] The present invention will be described in detail below in conjunction with specific embodiments. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention but are not intended to limit the present invention.

[0032] Unless otherwise specified, all of the following raw materials are commercially available or prepared by conventional methods in the art.

[0033] Ethylene-propylene copolymer comes from NS06 of Sino-Korea (Wuhan) Petrochemical; titanium dioxide comes from Chemours R105; antioxidant comes from BASF's B225; light stabilizer comes from BASF's 2020; maleic anhydride grafted polyolefin comes from DuPont's Fusabond P MD 353D; maleic anhydride grafted polypropylene wax comes from Clariant's LICOCENE PP MA 6452; high molecular weight epoxy resin comes from Nan Ya NPES-669; hydrogenated petroleum resin comes from Lanzhou Petrochemical's LH100-1.

[0034] Example 1

[0035] The TPO waterproofing membrane for metal-coated plates is composed of a polyolefin layer and an adhesive layer; the polyolefin layer is made of the following raw materials in parts by weight: 85 parts of ethylene-propylene copolymer, 5 parts of titanium dioxide, 10 parts of calcium carbonate, 0.4 parts of antioxidant, and 0.7 parts of light stabilizer; the adhesive layer is made of the following raw materials in parts by weight: 75 parts of maleic anhydride grafted polyolefin, 4 parts of maleic anhydride grafted polypropylene wax, 16 parts of high molecular weight epoxy resin, and 5 parts of hydrogenated petroleum resin. The thickness of the polyolefin layer is 1.5 mm, and the thickness of the adhesive layer is 100 μm.

[0036] The preparation method of Example 1 comprises the following steps:

[0037] S1. The ethylene-propylene copolymer, titanium dioxide, calcium carbonate, antioxidant and light stabilizer were weighed and added to a high-speed mixer at 480 r / min for dispersion for 30 min, and then transferred to a twin-screw extruder for granulation to obtain a polyolefin layer pellet for standby use. The temperature of the feeding section of the twin-screw extruder was 200 ° C, the temperatures of the three sections in the center of the screw were 210 ° C, 215 ° C, and 205 ° C, the die temperature was 200 ° C, and the screw speed was 400 r / min;

[0038] S2. The maleic anhydride grafted polyolefin, maleic anhydride grafted polypropylene wax, high molecular weight epoxy resin, and hydrogenated petroleum resin were weighed and added to a high-speed mixer at 480r / min for 30min, and then transferred to a twin-screw extruder for granulation to obtain a bonding layer of pellets for standby use. The temperature of the feeding section of the twin-screw extruder was 180°C, the temperatures of the three sections of the screw center were 190°C, 195°C, and 185°C, the die temperature was 180°C, and the screw speed was 200r / min;

[0039] S3. The polyolefin layer pellets obtained in step S1 are conveyed to the feeding hopper of extruder 1 of a multi-layer sheet screw extruder, and the bonding layer pellets obtained in step S2 are conveyed to the feeding hopper of extruder 2 of a multi-layer sheet screw extruder. After the temperatures of extruders 1 and 2 rise to the set temperatures, feeding begins. The thickness of the polyolefin layer is controlled to be 1.5 mm and the thickness of the bonding layer is controlled to be 100 μm by extrusion calendering to obtain a composite sheet consisting of a polyolefin layer and a bonding layer. The temperature of extruder 1 is set to: 110°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 208°C in zones 1-8, and continuous The temperature of the connection zone 1-3 is 210℃, 210℃, 210℃, the melt pump zone is 210℃, the mold zone 1-11 is 207℃, the left plate zone is 209℃, and the right plate zone is 209℃; the temperature setting of the extruder 2 is: 100℃, 160℃, 165℃, 170℃, 175℃, 180℃, 185℃, 188℃ in the 1-8 zone, 185℃, 185℃, 185℃ in the connection zone 1-3, 185℃, 185℃ in the melt pump zone, 187℃ in the mold zone 1-11, 189℃ in the left plate zone, and 189℃ in the right plate zone; the main engine speed of the multilayer sheet screw extruder is 24r / min, and the feeding speed ratio is 1;

[0040] S4. The composite sheet obtained in step S3 is cooled, trimmed, rolled and packaged to obtain a TPO waterproof membrane for metal-coated panels.

[0041] Example 2

[0042] The only difference from Example 1 is that the thickness of the adhesive layer is 150 μm.

[0043] Example 3

[0044] The only difference from Example 1 is that the thickness of the adhesive layer is 200 μm.

[0045] Comparative Example 1

[0046] The only difference from Example 1 is that the thickness of the adhesive layer is 50 μm.

[0047] Comparative Example 2

[0048] The only difference from Example 1 is that the raw materials of the adhesive layer do not include high molecular weight epoxy resin.

[0049] Comparative Example 3

[0050] The only difference from Example 1 is that the raw materials of the adhesive layer do not include high molecular weight epoxy resin and hydrogenated petroleum resin.

[0051] Experimental example:

[0052] The TPO waterproofing membranes prepared in Examples 1-3 and Comparative Examples 1-3 were respectively bonded to galvanized steel sheets to form metal-coated panels, and the preparation conditions were: temperature 200°C, pressure 0.8MPa, hot pressing time 2s, and the thickness of the galvanized steel sheet was 0.6mm; then the metal-coated panel was tested for peel strength at room temperature and peel strength at high temperature (70°C) according to the group standard T / CBMCA 017-2020 "Film-coated steel sheets for construction", and the results are shown in Table 1. In addition, a long-term boiling resistance test was added: the prepared metal-coated panel was gridded according to the adhesion test method, and the size of the grid was 3mm×3mm. Then the gridded metal-coated panel was boiled in boiling water for 500h according to this standard to observe whether there was bulging or shedding. The experimental results are shown in Table 1.

[0053] Table 1

[0054]

[0055] It can be seen from the experimental results in Table 1 that effective and reliable bonding can only be guaranteed when the thickness of the adhesive layer reaches 100μm or more. On the basis of rationally selecting the main resin of the adhesive layer, the adhesive layer with a certain proportion of high molecular epoxy resin and hydrogenated petroleum resin added has high room temperature peeling strength, high temperature peeling strength and excellent water boiling performance, thus ensuring the long-term durability of the system.

[0056] Example 4

[0057] The TPO waterproofing membrane used for metal-coated boards is composed of a polyolefin layer and an adhesive layer; the polyolefin layer is made of the following raw materials in parts by weight: 50 parts of ethylene-propylene copolymer, 4 parts of titanium dioxide, 8 parts of calcium carbonate, 0.1 parts of antioxidant, and 0.5 parts of light stabilizer; the adhesive layer is made of the following raw materials in parts by weight: 60 parts of maleic anhydride grafted polyolefin, 3 parts of maleic anhydride grafted polypropylene wax, 10 parts of high molecular weight epoxy resin, and 4 parts of hydrogenated petroleum resin. The thickness of the polyolefin layer is 0.5 mm, and the thickness of the adhesive layer is 100 μm.

[0058] The preparation method of Example 4 is different from that of Example 1 only in that the rotation speed of the high-speed stirrer in steps S1 and S2 is 400 r / min, and the thickness of the polyolefin layer is controlled to be 0.5 mm by extrusion calendering in step S3.

[0059] Example 5

[0060] The TPO waterproofing membrane used for metal-coated boards is composed of a polyolefin layer and an adhesive layer; the polyolefin layer is made of the following raw materials in parts by weight: 90 parts of ethylene-propylene copolymer, 10 parts of titanium dioxide, 20 parts of calcium carbonate, 0.5 parts of antioxidant, and 1 part of light stabilizer; the adhesive layer is made of the following raw materials in parts by weight: 90 parts of maleic anhydride grafted polyolefin, 8 parts of maleic anhydride grafted polypropylene wax, 20 parts of high molecular weight epoxy resin, and 10 parts of hydrogenated petroleum resin. The thickness of the polyolefin layer is 1.8 mm, and the thickness of the adhesive layer is 100 μm.

[0061] The preparation method of Example 5 is different from that of Example 1 only in that the rotation speed of the high-speed stirrer in steps S1 and S2 is 500 r / min, and the thickness of the polyolefin layer is controlled to be 1.8 mm by extrusion calendering in step S3.

[0062] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A TPO waterproofing membrane for metal coated boards, characterized in that: The invention is composed of a polyolefin layer and an adhesive layer; the polyolefin layer is made of the following raw materials in parts by weight: 50-90 parts of ethylene-propylene copolymer, 12-30 parts of filler, 0.1-0.5 parts of antioxidant and 0.5-1 parts of light stabilizer; the adhesive layer is made of the following raw materials in parts by weight: 60-90 parts of maleic anhydride grafted polyolefin, 3-8 parts of maleic anhydride grafted polypropylene wax, 10-20 parts of high molecular weight epoxy resin and 4-10 parts of hydrogenated petroleum resin.

2. The TPO waterproofing membrane for metal coated plates according to claim 1, characterized in that: The thickness of the polyolefin layer is 0.5-1.8 mm, and the thickness of the adhesive layer is 100-200 μm.

3. The TPO waterproof membrane for metal coated plates according to claim 1, characterized in that: The melt flow rate of the ethylene-propylene copolymer measured at 230° C. and 2.16 kg is 1-3 g / 10 min.

4. The TPO waterproof membrane for metal coated plates according to claim 1, characterized in that: The filler consists of titanium dioxide and calcium carbonate in a weight ratio of 1:

2.

5. The TPO waterproof membrane for metal coated plates according to claim 1, characterized in that: The maleic anhydride grafted polyolefin has a melt flow rate of 3-5 g / 10 min measured at 190° C. and 2.16 kg, and a maleic anhydride grafting rate of 1-5%.

6. The TPO waterproofing membrane for metal coated plates according to claim 1, characterized in that: The maleic anhydride grafted polypropylene wax has a softening point of 120-160° C. and an average molecular weight of 5000-20000.

7. The TPO waterproof membrane for metal coated plates according to claim 1, characterized in that: The epoxy equivalent of the high molecular weight epoxy resin is 2800-3500 and the softening point is 135-155°C.

8. The TPO waterproofing membrane for metal coated plates according to claim 1, characterized in that: The softening point of the hydrogenated petroleum resin is 100-130°C.

9. A method for preparing a TPO waterproof membrane for metal coated plates according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. The ethylene-propylene copolymer, filler, antioxidant, and light stabilizer were weighed and added to a high-speed mixer for dispersion for 30 min, and then transferred to a twin-screw extruder for granulation to obtain a polyolefin layer pellet for standby use; S2. The maleic anhydride grafted polyolefin, maleic anhydride grafted polypropylene wax, high molecular weight epoxy resin, hydrogenated petroleum resin were weighed and added to a high-speed mixer for dispersion for 30 min, and then transferred to a twin-screw extruder for granulation to obtain a bonding layer of pellets for standby; S3. The polyolefin layer pellets obtained in step S1 are conveyed to the feeding hopper of extruder 1 of the multi-layer sheet screw extruder, and the bonding layer pellets obtained in step S2 are conveyed to the feeding hopper of extruder 2 of the multi-layer sheet screw extruder, and the feeding is started after the temperature of extruder 1 and extruder 2 rises to the set temperature, and the composite sheet consisting of the polyolefin layer and the bonding layer is obtained by extrusion and calendaring; S4. The composite sheet obtained in step S3 is cooled, trimmed, rolled and packaged to obtain a TPO waterproof membrane for metal-coated panels.

10. The method for preparing a TPO waterproof membrane for a metal-faced plate according to claim 1, characterized in that: In step S1, the speed of the high-speed mixer is 400-500 r / min, the temperature of the feeding section of the twin-screw extruder is 200°C, the temperatures of the three sections in the center of the screw are 210°C, 215°C, and 205°C, the die temperature is 200°C, and the screw speed is 400 r / min; In step S2, the speed of the high-speed mixer is 400-500 r / min, the temperature of the feeding section of the twin-screw extruder is 180°C, the temperatures of the three sections in the center of the screw are 190°C, 195°C, and 185°C, the die temperature is 180°C, and the screw speed is 200 r / min; In the step S3, the temperature of the extruder 1 is set as follows: 110°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 208°C in zones 1-8, 210°C, 210°C, 210°C in zones 1-3, 210°C in melt pump zone, 207°C in zones 1-11 of the mold, 209°C in the left plate zone, and 209°C in the right plate zone; the temperature of the extruder 2 is set as follows: 100°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 188°C in zones 1-8, 185°C, 185°C, 185°C in zones 1-3, 185°C in melt pump zone, 187°C in zones 1-11 of the mold, 189°C in the left plate zone, and 189°C in the right plate zone; the main engine speed of the multilayer sheet screw extruder is 24r / min, and the feeding speed ratio is 1.

Citation Information

Patent Citations

  • Film-coated metal plate, preparation method and roof

    CN118082315A

Cited By

  • Non-asphalt-based waterproofing membrane and method for manufacturing the same

    CN122830219A