Waterproof sealant for cable and preparation method thereof

By using waterproof sealant composed of silane modified polymer and other components, the problem of poor waterproof material of cable joints is solved, the high-temperature durability and plastic peelability of the cable are achieved, the production process is simplified, and the overall performance of the cable is improved.

CN118978887AInactive Publication Date: 2024-11-19CAS APPLIED CHEM MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411154490.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing cable joint waterproof materials are not effective in cable joint applications, and cannot effectively prevent moisture infiltration, resulting in cable corrosion and reduced reliability. The cement has strong adhesive strength but complex peeling, and the secondary construction is complicated, which cannot meet the high temperature and high cables. Plasticity requirements.

Method used

The waterproof sealant consisting of silane modified polymer, dehydrating agent, moisture curing catalyst, silane coupling agent, inorganic filler, plasticizer and modified epoxy acrylate are used to form a waterproof sealant with a specific proportion of mixing and processing. Highly bonded and plastic sealant, suitable for waterproof sealing of cables.

Benefits of technology

The waterproof sealing effect of the cable is achieved, the sealant is resistant to high temperatures, has good plasticity, and is easy to peel off when necessary, simplifying the production process, reducing production energy consumption, and improving the overall performance of the cable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005004561460000101
    Figure BDA0005004561460000101
Patent Text Reader

Abstract

The invention relates to the technical field of cable sealants, in particular to a waterproof sealant for a cable and a preparation method of the waterproof sealant. The adhesive is composed of the following components in parts by weight: 25-50 parts of a silane modified polymer, 2-8 parts of a dehydrating agent, 0.5-2 parts of a moisture curing catalyst, 5-15 parts of a silane coupling agent, 10-22 parts of an inorganic filler, 2-18 parts of a plasticizer, 0.5-3 parts of tackifying resin and 10-40 parts of modified epoxy acrylate. The prepared sealant has waterproof and sealing effects, and has the advantages of high temperature resistance, good plasticity, easiness in stripping when necessary and the like when being used in cables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of cable sealants, and more specifically, to a waterproof sealant for cables and a preparation method thereof. Background Art

[0002] Cable joints are also called cable heads. After the cable is laid, in order to make it a continuous line, each section of the line must be connected as a whole, and these connection points are called cable joints. The cable joints in the middle of the cable line are called intermediate joints, and the cable joints at both ends of the line are called terminal heads. Cable joints are used to lock and fix the incoming and outgoing lines, and play a role in waterproofing, dustproofing and vibration prevention.

[0003] The main types of defects of power cable intermediate joints after long-term operation include horn cracking, water ingress into the joints, and corrosion of the aluminum sheath. Water ingress may cause corrosion of the aluminum sheath around the joint, causing insulation heating, and further deteriorating the reliability of cable operation; poor sealing will cause external water vapor and moisture to penetrate into the cable through the gap between the auxiliary equipment and the cable, eventually causing problems such as "water dendrites" and "electrochemical corrosion"; cables are immersed in water for a long time, especially when laying cables in some areas with harsh natural geographical environments and dense mountains and lakes, which will be directly damaged by geographical and geological factors.

[0004] Regarding waterproof materials, in the prior art, a patent document with publication number CN112694796A provides a composite waterproof coating, including liquid and powder, wherein the mass ratio of the liquid to powder is 1: (1-1.5); by weight, the liquid includes 30-50 parts of styrene-acrylic emulsion, 10-20 parts of nano-silicone-acrylic emulsion, 5-10 parts of epoxy-modified silicone resin emulsion, 0.5-1 part of dispersant, 0.4-0.8 parts of silicone defoamer, 0.4-0.6 parts of film-forming aid, 0.4-0.6 parts of thickener, and 20-30 parts of deionized water; by weight, the powder includes 30-50 parts of white cement, 10-20 parts of sodium metasilicate, and 10-20 parts of heavy calcium carbonate. The coating has good stability between the coating and concrete under sunlight exposure or salt freezing environment, and has high bonding strength and elongation at break on wet base surfaces. For another example, the patent document with publication number CN112375536A provides a waterproof elastic sealing material, including: liquid polysulfide rubber, with a number average molecular weight of 1000-7500 and a crosslinking degree of 0-2; the crosslinking agent is active manganese dioxide; the weight ratio of liquid polysulfide rubber to crosslinking agent is 6-14:1; the liquid polysulfide rubber accounts for 25-60% of the total weight of the waterproof elastic sealing material, and the crosslinking agent accounts for 2-5% of the total weight of the waterproof elastic sealing material. The caulking waterproof sealing material has a high mechanical property retention rate of bonding with concrete under long-term immersion conditions; it is suitable for improving the situation that the existing caulking sealing elastic material needs frequent maintenance due to the large attenuation of bonding strength under long-term immersion conditions, so as to improve the quality of waterproof projects, including tunnels, bridges, roads, sewage treatment pools, channels, etc. The above-mentioned waterproof materials are all used for bonding concrete, and the effect is not good in the waterproof sealing application of cable joints. Therefore, it is very necessary to improve the waterproof material so that it can be better applied to the waterproof sealing of cable joints and improve the overall performance of cables.

[0005] Among polymer putties, in addition to epoxy resin putty, there is also a type of polyurethane putty, which is a polymer-based putty formed by the polymerization of polyols and isocyanates. Polyurethane has excellent mechanical properties, is resistant to extrusion and stretching, and also has good plasticity, which is convenient for protecting and sealing various special-shaped materials; at the same time, polyurethane has good corrosion resistance and can maintain good weather resistance in acidic, alkaline, and high-salt conditions. For example, CN105061723A and CN105694796A respectively disclose a type of polyurethane putty, but generally this type of putty is mainly used for some materials with large sealing areas and volumes, such as buildings, ships, chimneys, and chemical pipelines.

[0006] The glue involved in the above prior art has strong bonding force and high strength after curing, but it cannot be peeled off immediately when needed, so the secondary construction is complicated during construction and the controllability is not high. Summary of the invention

[0007] The present invention discloses a waterproof sealant for cables and a preparation method thereof. The prepared sealant has a waterproof sealing effect. The sealant is used in cables and has the advantages of being resistant to high temperatures, having good plasticity, and being easy to peel off when necessary.

[0008] In a first aspect, the present disclosure provides a waterproof sealant for cables, comprising the following components in parts by weight:

[0009] Silane modified polymer 25-50 parts,

[0010] 2-8 parts of dehydrating agent,

[0011] Moisture curing catalyst 0.5-2 parts,

[0012] Silane coupling agent 5-15 parts,

[0013] Inorganic filler 10-22 parts,

[0014] Plasticizer 2-18 parts,

[0015] 0.5-3 parts of tackifying resin,

[0016] Modified epoxy acrylate 10-40 parts.

[0017] Preferably, it is composed of the following ingredients in parts by weight:

[0018] Silane modified polymer 35-50 parts,

[0019] 2-5 parts of dehydrating agent,

[0020] 1-2 parts of moisture curing catalyst,

[0021] Silane coupling agent 10-15 parts,

[0022] Inorganic filler 10-18 parts,

[0023] 8-16 parts of plasticizer,

[0024] 1.5-3 parts of tackifying resin,

[0025] Modified epoxy acrylate 28-40 parts.

[0026] Preferably, it is composed of the following ingredients in parts by weight:

[0027] Silane modified polymer 40-48 parts,

[0028] 3-6 parts of dehydrating agent,

[0029] 1-1.5 parts of moisture curing catalyst,

[0030] Silane coupling agent 8-10 parts,

[0031] Inorganic filler 18-20 parts,

[0032] 8-10 parts of plasticizer,

[0033] 2-3 parts of tackifying resin,

[0034] Modified epoxy acrylate 20-30 parts.

[0035] Preferably, the silane-modified polymer is composed of the following components in parts by weight: 10-25 parts of epoxidized vegetable oil, 21-45 parts of silane-modified polyether, and 5-10 parts of vinyl silane.

[0036] Preferably, the silane-modified polymer is composed of the following components in parts by weight: 10-15 parts of epoxidized vegetable oil, 21-32 parts of silane-modified polyether, and 5-8 parts of vinyl silane.

[0037] Preferably, the silane-modified polymer is composed of the following components in parts by weight: 15-20 parts of epoxidized vegetable oil, 21-28 parts of silane-modified polyether, and 5-6 parts of vinyl silane.

[0038] Preferably, the inorganic filler is one or more of nano copper oxide, CaCO3@ZnO, and CaCO3@TiO2.

[0039] Preferably, the silane-modified polymer is prepared by mixing epoxidized vegetable oil, silane-modified polyether and vinyl silane, and the epoxidized vegetable oil is a mixture of one or more of epoxidized soybean oil, epoxidized castor oil, epoxidized palm oil, epoxidized linseed oil and epoxidized sunflower oil.

[0040] Preferably, the silane-modified polymer is prepared by stirring and mixing epoxidized vegetable oil and silane-modified polyether at a temperature of 45-60° C., and then adding vinyl silane and stirring and mixing at a rotation speed of 3000-5000 rpm to obtain the silane-modified polymer.

[0041] Preferably, the modified epoxy acrylate is prepared by modifying epoxy resin with polyethylene glycol and polyimide to generate modified epoxy resin, reacting the modified epoxy resin with acrylic acid to obtain epoxy acrylate resin, introducing succinic anhydride groups into the epoxy acrylate resin, neutralizing with triethylamine to form a salt, and emulsifying with water to synthesize modified epoxy acrylate.

[0042] Preferably, the mass ratio of the polyethylene glycol to the polyimide is 1-3:2-5.

[0043] Preferably, the mass ratio of the polyethylene glycol to the polyimide is 3:5.

[0044] Preferably, the dehydrating agent is one of vinyltrimethoxysilane and dimethoxydiphenylsilane.

[0045] Preferably, the moisture curing catalyst is one or more of dimethylethanolamine, methyldiethanolamine, tetrakis(2-hydroxypropyl)ethylenediamine, N-ethylmorpholine, dibutyltin dilaurate, cobalt cyclopentaneate, calcium cyclopentaneate and lead cyclopentaneate; the best choice of silane coupling agent is KH792.

[0046] Preferably, the plasticizer is one of chloromethoxy fatty acid methyl ester, acetyl tributyl citrate, dibutyl diglyceride adipate, dioctyl phthalate, and dibutyl phthalate.

[0047] In a second aspect, the present disclosure provides a method for preparing a waterproof sealant for a cable, comprising the following steps:

[0048] (1) mixing a silane-modified polymer, a moisture-curing catalyst, and a silane coupling agent, heating to 30-40° C., and slowly stirring for 40-50 minutes to obtain a first mixture;

[0049] (2) keeping the temperature constant, adding modified epoxy acrylate and plasticizer to the first mixture, stirring for 30-40 minutes, to obtain a second mixture;

[0050] (3) Keeping the temperature constant, adding a dehydrating agent, an inorganic filler and a tackifying resin into the second mixture, stirring rapidly, and standing to cool, thereby obtaining a waterproof sealant.

[0051] In summary, this application has the following beneficial effects:

[0052] 1. The silane-modified polymer in this application is a high-performance environmentally friendly polymer, which has the advantages of both polyurethane sealant and silicone sealant, has excellent mechanical properties, good adhesion, and environmental friendliness, realizes the integrated process of silane-modified polymer and its sealant, has a simple preparation method, is easy to operate, has low production cost, and is easy to industrialize;

[0053] 2. In this application, groups in the resin, such as epoxy groups and hydroxyl groups, are used to introduce soft chains or hard chains, thereby improving the viscosity of the resin and enhancing the flexibility and adhesion of the coating; inorganic fillers are added to the polymer as light shielding agents to improve the aging resistance of the polymer;

[0054] 3. The present application uses silane-modified polymer as the main rubber material, and mixes it with moisture-curing catalyst, silane coupling agent, tackifying resin, modified epoxy acrylate, plasticizer, inorganic filler and other components in a certain proportion to form a viscous composition with good fluidity. It does not need to maintain high-temperature mixing and shearing for a long time, and can be formed into a film by simple coating afterwards, which greatly simplifies the production process and reduces production energy consumption.

[0055] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not intended to limit the scope of protection of the present disclosure. DETAILED DESCRIPTION

[0056] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0057] Preparation examples of raw materials and / or intermediates

[0058] Preparation Example 1

[0059] A silane-modified polymer is composed of the following ingredients in parts by weight: 10 g of epoxidized vegetable oil, 21 g of silane-modified polyether and 5 g of vinyl silane.

[0060] A method for preparing a silane-modified polymer comprises the following steps:

[0061] (1) Epoxy castor oil and silane-modified polyether are stirred and mixed uniformly at a temperature of 45° C.;

[0062] (2) Vinyl silane was added and stirred at a speed of 5000 rpm to obtain a silane-modified polymer.

[0063] Preparation Example 2

[0064] A silane-modified polymer is composed of the following ingredients in parts by weight: 15 g of epoxidized vegetable oil, 35 g of silane-modified polyether and 8 g of vinyl silane.

[0065] A method for preparing a silane-modified polymer comprises the following steps:

[0066] (1) Epoxy palm oil and silane-modified polyether are stirred and mixed at a temperature of 50° C.

[0067] (2) Vinyl silane was added and stirred at a speed of 5000 rpm to obtain a silane-modified polymer.

[0068] Preparation Example 3

[0069] A silane-modified polymer is composed of the following ingredients in parts by weight: 25 g of epoxidized vegetable oil, 45 g of silane-modified polyether and 10 g of vinyl silane.

[0070] A method for preparing a silane-modified polymer comprises the following steps:

[0071] (1) Epoxy linseed oil and silane-modified polyether are stirred and mixed uniformly at a temperature of 60° C.;

[0072] (2) Vinyl silane was added and stirred at a speed of 5000 rpm to obtain a silane-modified polymer.

[0073] Preparation Example 4

[0074] A method for preparing modified epoxy acrylate comprises the following steps:

[0075] (1) modifying epoxy resin with polyethylene glycol and polyimide, wherein the mass ratio of polyethylene glycol to polyimide is 3:5, to generate modified epoxy resin;

[0076] (2) reacting the modified epoxy resin with acrylic acid, wherein the mass ratio of the modified epoxy resin to the acrylic acid is 1:2, to obtain an epoxy acrylate resin;

[0077] (3) 30 mL of succinic anhydride was introduced into the epoxy acrylate resin, neutralized with 60 mL of triethylamine to form a salt, and emulsified with 100 mL of water to synthesize modified epoxy acrylate.

[0078] Preparation Example 5

[0079] A method for preparing modified epoxy acrylate comprises the following steps:

[0080] (1) modifying epoxy resin with polyethylene glycol and polyimide, wherein the mass ratio of polyethylene glycol to polyimide is 1:5, to generate modified epoxy resin;

[0081] (2) reacting the modified epoxy resin with acrylic acid, wherein the mass ratio of the modified epoxy resin to the acrylic acid is 1:3, to obtain an epoxy acrylate resin;

[0082] (3) 30 mL of succinic anhydride was introduced into the epoxy acrylate resin, neutralized with 60 mL of triethylamine to form a salt, and emulsified with 100 mL of water to synthesize modified epoxy acrylate.

[0083] Preparation Example 6

[0084] A method for preparing modified epoxy acrylate comprises the following steps:

[0085] (1) modifying epoxy resin with polyethylene glycol and polyimide, wherein the mass ratio of polyethylene glycol to polyimide is 2:3, to generate modified epoxy resin;

[0086] (2) reacting the modified epoxy resin with acrylic acid, wherein the mass ratio of the modified epoxy resin to the acrylic acid is 1:1, to obtain an epoxy acrylate resin;

[0087] (3) 30 mL of succinic anhydride was introduced into the epoxy acrylate resin, neutralized with 60 mL of triethylamine to form a salt, and emulsified with 100 mL of water to synthesize modified epoxy acrylate.

[0088] Example

[0089] Example 1

[0090] A waterproof sealant for cables, comprising the following components in parts by weight:

[0091] Silane modified polymer 25g, dehydrating agent 2g, moisture curing catalyst 0.5g, silane coupling agent 5g, inorganic filler 10g, plasticizer 2g, tackifying resin 0.5g, modified epoxy acrylate 10g;

[0092] The silane-modified polymer was prepared in Preparation Example 1;

[0093] The dehydrating agent is vinyltrimethoxysilane;

[0094] The moisture curing catalyst is a mixture of tetrakis(2-hydroxypropyl)ethylenediamine and N-ethylmorpholine in a mass ratio of 1:1;

[0095] The silane coupling agent is KH792;

[0096] The inorganic filler is CaCO3@ZnO;

[0097] The plasticizer is chloromethoxy fatty acid methyl ester;

[0098] The modified epoxy acrylate was prepared in Preparation Example 4.

[0099] A method for preparing a waterproof sealant for a cable comprises the following steps:

[0100] (1) mixing a silane-modified polymer, a moisture-curing catalyst, and a silane coupling agent, heating to 30° C., and slowly stirring for 40 minutes to obtain a first mixture;

[0101] (2) keeping the temperature constant, adding the modified epoxy acrylate and the plasticizer to the first mixture, stirring for 30 minutes, to obtain a second mixture;

[0102] (3) Keeping the temperature constant, add a dehydrating agent, an inorganic filler and a tackifying resin into the second mixture, stir rapidly, and allow to cool to obtain a waterproof sealant.

[0103] Example 2

[0104] A waterproof sealant for cables, comprising the following components in parts by weight:

[0105] Silane modified polymer 36g, dehydrating agent 5g, moisture curing catalyst 1g, silane coupling agent 10g, inorganic filler 16g, plasticizer 9g, tackifying resin 2g, modified epoxy acrylate 25g;

[0106] The silane-modified polymer was prepared in Preparation Example 2;

[0107] The dehydrating agent is dimethoxydiphenylsilane;

[0108] The moisture curing catalyst is methyldiethanolamine;

[0109] The silane coupling agent is KH792;

[0110] The inorganic filler is CaCO3@TiO2;

[0111] The plasticizer is acetyl tributyl citrate;

[0112] The modified epoxy acrylate was prepared in Preparation Example 5.

[0113] A method for preparing a waterproof sealant for a cable comprises the following steps:

[0114] (1) mixing a silane-modified polymer, a moisture-curing catalyst, and a silane coupling agent, heating to 40° C., and slowly stirring for 40 minutes to obtain a first mixture;

[0115] (2) keeping the temperature constant, adding the modified epoxy acrylate and the plasticizer to the first mixture, stirring for 30 minutes, to obtain a second mixture;

[0116] (3) Keeping the temperature constant, add a dehydrating agent, an inorganic filler and a tackifying resin into the second mixture, stir rapidly, and allow to cool to obtain a waterproof sealant.

[0117] Example 3

[0118] A waterproof sealant for cables, comprising the following components in parts by weight:

[0119] Silane modified polymer 50g, dehydrating agent 8g, moisture curing catalyst 2g, silane coupling agent 15g, inorganic filler 22g, plasticizer 18g, tackifying resin 3g, modified epoxy acrylate 40g;

[0120] The silane-modified polymer was prepared in Preparation Example 3;

[0121] The dehydrating agent is vinyltrimethoxysilane;

[0122] The moisture curing catalyst is dimethylethanolamine;

[0123] The silane coupling agent is KH792;

[0124] The inorganic filler is nano copper oxide;

[0125] The plasticizer is dibutyl diglyceride;

[0126] The modified epoxy acrylate was prepared in Preparation Example 6.

[0127] A method for preparing a waterproof sealant for a cable comprises the following steps:

[0128] (1) mixing a silane-modified polymer, a moisture-curing catalyst, and a silane coupling agent, heating to 40° C., and slowly stirring for 45 minutes to obtain a first mixture;

[0129] (2) keeping the temperature constant, adding the modified epoxy acrylate and the plasticizer to the first mixture, stirring for 35 minutes, to obtain a second mixture;

[0130] (3) Keeping the temperature constant, add a dehydrating agent, an inorganic filler and a tackifying resin into the second mixture, stir rapidly, and allow to cool to obtain a waterproof sealant.

[0131] Comparative Example

[0132] Comparative Example 1

[0133] A waterproof sealant for cables was prepared according to the method of Example 2, except that no silane-modified polymer was added.

[0134] Comparative Example 2

[0135] A waterproof sealant for cables was prepared according to the method of Example 2, except that no inorganic filler was added.

[0136] Comparative Example 3

[0137] A waterproof sealant for cables was prepared according to the method of Example 2, except that the inorganic filler was replaced by titanium dioxide.

[0138] Comparative Example 4

[0139] A waterproof sealant for cables was prepared according to the method of Example 2, except that no modified epoxy acrylate was added.

[0140] According to the JC / T942-2004 standard for waterproof sealants for cables and the national standard GB55030-2022, the waterproof sealants prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to performance tests and water-tightness tests, respectively. The results are shown in Table 1.

[0141]

[0142] The test results in Table 1 show that the waterproof sealant for cables prepared by the present invention has the effect of waterproof sealing, and the sealant is resistant to high temperatures in cables, has good plasticity, and is easy to peel off when necessary. Among them, the waterproof sealant for cables prepared in Example 2 has the best performance, indicating that the groups in the resin, such as epoxy groups and hydroxyl groups, are used to introduce soft chains or hard chains, thereby improving the viscosity of the resin, and enhancing the flexibility and adhesion of the coating, and the performance is more prominent in the sealant.

[0143] The above is only an exemplary embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present disclosure should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. A waterproof sealant for cables, It is characterized in that It is composed of the following ingredients in parts by weight: Silane modified polymer 25-50 parts, 2-8 parts of dehydrating agent, Moisture curing catalyst 0.5-2 parts, Silane coupling agent 5-15 parts, Inorganic filler 10-22 parts, Plasticizer 2-18 parts, 0.5-3 parts of tackifying resin, Modified epoxy acrylate 10-40 parts.

2. The waterproof sealant for cables according to claim 1, It is characterized in that The silane-modified polymer is composed of the following components in parts by weight: 10-25 parts of epoxidized vegetable oil, 21-45 parts of silane-modified polyether, and 5-10 parts of vinyl silane.

3. The waterproof sealant for cables according to claim 1, It is characterized in that The inorganic filler is nano copper oxide, CaCO 3 @ZnO, CaCO 3 @TiO 2 One or more of .

4. The waterproof sealant for cables according to claim 2, It is characterized in that The silane-modified polymer is prepared by mixing epoxidized vegetable oil, silane-modified polyether and vinyl silane. The epoxidized vegetable oil is a mixture of one or more of epoxidized soybean oil, epoxidized castor oil, epoxidized palm oil, epoxidized linseed oil and epoxidized sunflower oil.

5. The waterproof sealant for cables according to claim 1, It is characterized in that The modified epoxy acrylate is prepared by modifying epoxy resin with polyethylene glycol and polyimide to generate modified epoxy resin, reacting the modified epoxy resin with acrylic acid to obtain epoxy acrylate resin, introducing succinic anhydride groups into the epoxy acrylate resin, neutralizing with triethylamine to form salt, and emulsifying with water to synthesize the modified epoxy acrylate.

6. The waterproof sealant for cables according to claim 5, It is characterized in that The mass ratio of the polyethylene glycol to the polyimide is 1-3:2-5.

7. The waterproof sealant for cables according to claim 1, It is characterized in that The dehydrating agent is one of vinyltrimethoxysilane and dimethoxydiphenylsilane.

8. The waterproof sealant for cables according to claim 1, It is characterized in that The moisture curing catalyst is one or more of dimethylethanolamine, methyldiethanolamine, tetrakis(2-hydroxypropyl)ethylenediamine, N-ethylmorpholine, dibutyltin dilaurate, cobalt naphthenate, calcium naphthenate, and lead naphthenate.

9. The waterproof sealant for cables according to claim 1, It is characterized in that The plasticizer is one of chloromethoxy fatty acid methyl ester, acetyl tributyl citrate, dibutyl diglyceride adipate, dioctyl phthalate, and dibutyl phthalate.

10. A method for preparing a waterproof sealant for cables according to any one of claims 1 to 9, It is characterized in that The following steps are involved: (1) mixing a silane-modified polymer, a moisture-curing catalyst, and a silane coupling agent, heating to 30-40° C., and slowly stirring for 40-50 minutes to obtain a first mixture; (2) keeping the temperature constant, adding modified epoxy acrylate and plasticizer to the first mixture, stirring for 30-40 minutes, to obtain a second mixture; (3) Keeping the temperature constant, adding a dehydrating agent, an inorganic filler and a tackifying resin into the second mixture, stirring rapidly, and standing to cool, thereby obtaining a waterproof sealant.

Citation Information

Patent Citations

  • PU (polyurethane) daub and preparation method thereof

    CN105061723A

  • Polyurethane-modified daub for leaking stoppage

    CN105694796A

  • Waterproof elastic sealing material

    CN112375536A

  • Composite waterproof coating and preparation method thereof

    CN112694796A