Red fluorescent powder of europium-doped fluorapatite and preparation method of red fluorescent powder
By introducing Eu3+ doping into fluorapatite, europium-doped fluorapatite red phosphor was prepared, which solved the high cost and environmental problems in the preparation process of existing red phosphors, and achieved low correlation color temperature and high color development index The white LED has excellent optical performance and stability.
Patent Information
- Application Number
- CN202411228288.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-03
AI Technical Summary
During the preparation process, existing red phosphors have high costs, high temperature and high pressure requirements, unfriendly environment and photon reabsorption problems, resulting in high color temperature and low color rendering index of white LEDs, making it difficult to achieve low correlation color temperature and high color rendering index.
Using europium-doped fluorapatite red phosphor, the phosphor that exhibits narrow band red emission under ultraviolet to blue light excitation is prepared by introducing Eu3+ activator into the fluorapatite lattice. The chemical formula is Ca10-xEux ( PO4)6F2, 0.02≤x≤0.2, synthesis is performed by stoichiometric ratio, including weighing raw materials, mixing, stirring, heating and cleaning.
Achieved environmentally friendly and low-cost red phosphor, with color temperature maintained at 2138.74K, color purity up to 86.95%, low thermal quenching activation energy, excellent fluorescence intensity, good physical and chemical stability and anti-thermal quenching performance .
Smart Images

Figure CN118978915A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of luminescent materials, and in particular to a preparation method of europium-doped fluoroapatite red phosphor and application thereof. Background Art
[0002] LED lighting is a lighting technology based on semiconductor chips that convert electrical energy into light energy. It has the advantages of high conversion efficiency, long life, green environmental protection, adjustable light intensity, rich colors, etc. At present, white light LED is mainly used in solid-state lighting. The specific principle is to combine blue light with a wavelength of 460nm with YAG:Ce that can convert part of blue light into yellow light. 3+ However, the blue light chip excites YAG:Ce 3+ The white light formed by the phosphor has problems such as high color temperature, low color rendering index, and poor color reproduction. Therefore, it is of great significance to prepare a red phosphor with excellent performance to achieve white light LED with low correlated color temperature and high color rendering index.
[0003] At present, the main red phosphor is Eu 2+ Doping with nitride, oxynitride or sulfide and Mn 4+ Doped fluoride phosphors are mainly used. 2+ Doped nitrides have rich luminous colors, high luminous efficiency, and low thermal quenching performance, but nitride-based phosphors need to be prepared in high temperature, high pressure and inert gas, which is costly, and the stimulated emission has a wide wavelength band, with severe photon reabsorption in the green and yellow regions, resulting in a reduction in the short wavelength component in white light LEDs. 2+ Doped sulfides have higher luminescence efficiency and better temperature stability, but the presence of the sulfide matrix will produce harmful substances during the preparation process, which is not environmentally friendly. 4+ Fluoride-doped materials have weak luminescence intensity and poor thermal stability, and Mn 4+ The chemical stability of Mn in fluoride is relatively poor. In a humid environment, 4+ It is easy to hydrolyze into manganese oxide and hydroxide, resulting in reduced luminous efficiency of the phosphor. Therefore, it is necessary to develop a red phosphor that is environmentally friendly, low-cost, has excellent optical properties, and is easy to produce and prepare. Summary of the invention
[0004] The object of the present invention is to provide a europium-doped fluoroapatite and a preparation method thereof. The phosphor is environmentally friendly, low in cost, has excellent optical properties, is easy to prepare, and can be used to generate a fluorescent substance under ultraviolet to blue light excitation. 3+In the fluoroapatite lattice, it exhibits strong narrow-band red emission, with an emission wavelength range of 579-696nm and a main peak at 618nm. Calculations show that its color temperature remains at 2138.74K, the color purity is 86.95%, and the thermal quenching activation energy is 0.276eV, indicating that europium-doped fluoroapatite is a red phosphor with high color saturation, good thermal stability, and excellent fluorescence intensity.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A europium-doped apatite-based red phosphor, the chemical formula of which is Ca 10-x Eu x (PO4)6F2, where the activator is Eu 3 + , 0.02≤x≤0.2.
[0007] A method for preparing europium-doped fluoroapatite red phosphor comprises the following steps:
[0008] Step 1: weigh the raw materials containing Ca and Eu and cetyltrimethylammonium bromide according to the stoichiometric ratio and mix them evenly to form solution A, weigh the raw materials containing F and PO4 and sodium citrate and mix them evenly to form solution B;
[0009] Step 2: Add solution B dropwise into solution A and stir evenly;
[0010] Step 3: Place the mixed solution into a reactor, heat it, cool it, and then wash and dry it;
[0011] Preferably, the stoichiometric ratio of Ca, Eu, F, PO4, hexadecyltrimethylammonium bromide and sodium citrate is 0.37:1:0.41:0.11:1.
[0012] Preferably, the Ca-containing compound is any one of calcium chloride, calcium nitrate, calcium acetate, calcium sulfate, and calcium bicarbonate, or a combination of at least two thereof.
[0013] Preferably, the F-containing compound is a soluble fluoride such as sodium fluoride, potassium fluoride, ammonium fluoride, lithium fluoride, or ammonium bifluoride.
[0014] Preferably, the phosphate is a soluble phosphate such as potassium dihydrogen phosphate, sodium dihydrogen phosphate, sodium tripolyphosphate, sodium pyrophosphate, sodium hexametaphosphate, etc.
[0015] Preferably, the stirring method is magnetic stirring, the stirring speed is 500±50r / min, and the stirring time is 50 to 120 minutes.
[0016] Preferably, the heating device may be an oven, the heating container may be a reactor, and the heating temperature may be 150 to 250°C.
[0017] Preferably, the cleaning solvents are deionized water and anhydrous ethanol.
[0018] Beneficial results of the present invention:
[0019] 1. The phosphor prepared by the present invention can be effectively excited in the 200-480nm band, the emission wavelength range is 575-700nm, and the main peak is located at 600-630nm.
[0020] 2. The phosphor prepared by the present invention has good resistance to thermal quenching, and the main peak fluorescence intensity of the emission peak at 448K can still maintain about 80% of the initial value.
[0021] 3. The phosphor prepared by the present invention has excellent physical and chemical stability and is very environmentally friendly because it is an apatite-based phosphor. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The Ca prepared in Example 1 0.92 Eu 0.08 X-ray diffraction pattern of (PO4)6F2 sample.
[0023] Figure 2 The Ca prepared in Example 1 0.92 Eu 0.08 Scanning electron micrograph of a (PO4)6F2 sample.
[0024] Figure 3 The Ca prepared in Example 1 0.92 Eu 0.08 Photoluminescence spectrum of (PO4)6F2 sample.
[0025] Figure 4 The Ca prepared in Example 2 0.9 Eu 0.1 X-ray diffraction pattern of (PO4)6F2 sample.
[0026] Figure 5 The Ca prepared in Example 1 0.9 Eu 0.1 Scanning electron micrograph of a (PO4)6F2 sample.
[0027] Figure 6 The Ca prepared in Example 2 0.9 Eu 0.1 Photoluminescence spectrum of (PO4)6F2 sample.
[0028] Figure 7 The Ca prepared in Example 3 0.88 Eu0.12 X-ray diffraction pattern of (PO4)6F2 sample.
[0029] Figure 8 The Ca prepared in Example 1 0.88 Eu 0.12 Scanning electron micrograph of a (PO4)6F2 sample.
[0030] Fig. 9 The Ca prepared in Example 3 0.88 Eu 0.12 Photoluminescence spectrum of (PO4)6F2 sample. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be noted that these embodiments are only used to illustrate the present invention and do not limit the scope of the present invention.
[0032] Example 1
[0033] Preparation of Ca 0.92 Eu 0.08 (PO4)6F2 sample: First, mix 81.09g of Ca(NO3)2·4H2O, 13.2g of Eu(NO3)3, and 40.2g of hexadecyltrimethylammonium bromide evenly with 500mL of deionized water to form solution A; mix 41.99g of NaF, 54.14g of (NH4)2HPO4, and 25.8g of Na3Cit evenly with 500mL of deionized water solution B. Next, add solution B into solution A at a rate of 10 drops per minute, and stir at 500r / min for 30 minutes using a magnetic stirrer; transfer the mixed solution to the reactor and place it in an oven, adjust the temperature to 180°C and heat for 12 hours. Finally, wash the resulting powder twice with anhydrous ethanol and deionized water respectively, and then place it in a vacuum drying oven and dry it at 80°C to obtain Ca 0.92 Eu 0.08 (PO4)6F2 crystals.
[0034] The prepared Ca 0.92 Eu 0.08 (PO4)6F2 crystals were subjected to X-ray diffraction analysis, such as Figure 1 As shown in the figure, the XRD diffraction peaks of the obtained powder crystals completely correspond to the pure fluoroapatite phase, and no impurity peaks appear, indicating that the prepared sample is a pure phase. In addition, the experimental samples were subjected to scanning electron microscopy micromorphology analysis. Figure 2The obtained particles have a rod-like morphology, with an average length of about 3-4 μm and an average diameter of about 1-2 μm. Under the excitation of 250 μm, the emission spectrum of the sample powder is as follows Figure 3 As shown, five diffraction peaks appear in the band from 575 to 750 nm, corresponding to 5 D0→ 7 F0, 5 D0→ 7 F1, 5 D0→ 7 F2, 5 D0→ 7 F3, 5 D0→ 7 F4 transition eventually shows that the fluorescence emits red light.
[0035] Example 2
[0036] Preparation of Ca 0.9 Eu 0.1 (PO4)6F2 sample: First, mix 79.31g of Ca(NO3)2·4H2O, 16.5g of Eu(NO3)3, and 40.2g of hexadecyltrimethylammonium bromide evenly with 500mL of deionized water to form solution A; mix 41.99g of NaF, 54.14g of (NH4)2HPO4, and 25.8g of Na3Cit evenly with 500mL of deionized water solution B. Next, add solution B into solution A at a rate of 10 drops per minute, and stir at 500r / min for 30 minutes using a magnetic stirrer; transfer the mixed solution to the reactor and place it in an oven, adjust the temperature to 180°C and heat for 12 hours. Finally, wash the resulting powder twice with anhydrous ethanol and deionized water respectively, and then place it in a vacuum drying oven and dry it at 80°C to obtain Ca 0.9 Eu 0.1 (PO4)6F2 crystals.
[0037] The prepared Ca 0.9 Eu 0.1 (PO4)6F2 crystals were subjected to X-ray diffraction analysis, such as Figure 4 As shown in the figure, the XRD diffraction peaks of the obtained powder crystals completely correspond to the pure fluoroapatite phase, and no impurity peaks appear, indicating that the prepared sample is a pure phase. In addition, the experimental samples were subjected to scanning electron microscopy micromorphology analysis. Figure 5 The obtained particles have a rod-like morphology, with an average length of about 3-4 μm and an average diameter of about 1-2 μm. Under the excitation of 250 μm, the emission spectrum of the sample powder is as follows Figure 6 As shown, five diffraction peaks appear in the band from 575 to 750 nm, corresponding to 5 D0→7 F0, 5 D0→ 7 F1, 5 D0→ 7 F2, 5 D0→ 7 F3, 5 D0→ 7 F4 transition eventually shows that the fluorescence emits red light.
[0038] Example 3
[0039] Preparation of Ca 0.88 Eu 0.12 (PO4)6F2 sample: First, mix 77.55g of Ca(NO3)2·4H2O, 19.8g of Eu(NO3)3, and 40.2g of hexadecyltrimethylammonium bromide evenly with 500mL of deionized water to form solution A; mix 41.99g of NaF, 54.14g of (NH4)2HPO4, and 25.8g of Na3Cit evenly with 500mL of deionized water solution B. Next, add solution B into solution A at a rate of 10 drops per minute, and stir at 500r / min for 30 minutes using a magnetic stirrer; transfer the mixed solution to the reactor and place it in an oven, adjust the temperature to 180°C and heat for 12 hours. Finally, wash the resulting powder twice with anhydrous ethanol and deionized water respectively, and then place it in a vacuum drying oven and dry it at 80°C to obtain Ca 0.88 Eu 0.12 (PO4)6F2 crystals.
[0040] The prepared Ca 0.88 Eu 0.12 (PO4)6F2 crystals were subjected to X-ray diffraction analysis, such as Figure 7 As shown in the figure, the XRD diffraction peaks of the obtained powder crystals completely correspond to the pure fluoroapatite phase, and no impurity peaks appear, indicating that the prepared sample is a pure phase. In addition, the experimental samples were subjected to scanning electron microscopy micromorphology analysis. Figure 8 The obtained particles have a rod-like morphology, with an average length of about 3-4 μm and an average diameter of about 1-2 μm. Under the excitation of 250 μm, the emission spectrum of the sample powder is as follows Fig. 9 As shown, five diffraction peaks appear in the band from 575 to 750 nm, corresponding to 5 D0→ 7 F0, 5 D0→ 7 F1, 5 D0→ 7 F2, 5 D0→ 7 F3, 5D0→ 7 F4 transition eventually shows that the fluorescence emits red light.
Claims
1. A europium-doped apatite-based red phosphor, characterized in that: The general formula of the apatite-based phosphor is Ca10-xEux(PO4)6F2, wherein: The matrix is Ca10(PO4)6F2, and the activator is Eu3+, which is obtained by replacing the cations in the matrix with Eu3+; 0.02≤x≤0.2; The phosphor Ca10-xEux(PO4)6X2 is prepared via a hydrothermal synthesis method.
2. A method for preparing europium-doped apatite-based red phosphor, using a hydrothermal synthesis method, characterized in that: The following steps are involved: Step 1, weighing a calcium source, hexadecyltrimethylammonium bromide, and a Eu3+-containing compound in a stoichiometric ratio and mixing them uniformly to form a solution A, and weighing corresponding amounts of sodium citrate, fluoride, and phosphate and mixing them uniformly to form a solution B; Step 2, add solution B into solution A and stir evenly; Step 3, the mixed solution is placed in a reaction kettle, heated, cooled, and then cleaned and dried.
3. The preparation method according to claim 1, characterized in that: In the step 1, the stoichiometric ratio of Ca and Eu, F, PO4, hexadecyltrimethylammonium bromide and sodium citrate is 0.37:1:0.41:0.11:
1.
4. The preparation method according to claim 1, characterized in that: In step 1, the calcium source includes: one or more of calcium chloride, calcium nitrate, calcium acetate, calcium sulfate or calcium bicarbonate; the compound containing Eu3+ includes one or more of europium nitrate or europium acetate; the fluoride includes one or more of sodium fluoride, potassium fluoride, ammonium fluoride, lithium fluoride or ammonium bifluoride; the phosphate includes one or more of potassium dihydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium tripolyphosphate, sodium pyrophosphate, and sodium hexametaphosphate.
5. The preparation method according to claim 1, characterized in that: In the step 2, solution B is added to solution A by dropwise addition.
6. The preparation method according to claim 1, characterized in that: In the step 2, the stirring method is magnetic stirring, the stirring speed is 500±50 r / min, and the stirring time is 50 to 120 minutes.
7. The preparation method according to claim 1, characterized in that: In the step 3, the reactor is heated for 5 to 10 hours at a heating temperature of 150 to 250°C.
8. The preparation method according to claim 1, characterized in that: In the step 3, the cleaning solvents are deionized water and anhydrous ethanol.
9. The preparation method according to claim 1, characterized in that: The range of the excitation spectrum is 200-480nm, the range of the emission spectrum is 575-700nm, the main emission peak is in the range of 600-630nm, and the emitted light is red light.
10. The preparation method according to claim 1, characterized in that: Eu3+ doped apatite-based phosphors are used in solid-state lighting and display fields.
Citation Information
Patent Citations
Phosphate red fluorescent powder excited by blue light and preparation method thereof
CN102994081A
Europium ion activated phosphate red fluorescent powder and preparation method thereof
CN103694999A
Europium-doped red phosphor taking phosphate as matrix and preparation method of red phosphor
CN107312542A
Preparation method of red europium-doped lanthanum molybdate fluorescent powder
CN108276999A
Red phosphor activated by europium ions Eu3+, preparation method and application
CN109777421A
Cited By
Red light-emitting material of beta-diketone Schiff base europium-zinc complex as well as preparation method and application of red light-emitting material
CN120040519A
Synthesis method of apatite type fluorescent powder
CN120041200A