High-capacity fast-charging needle coke for lithium ion battery negative electrode material

By optimizing the polarization structure and electrochemical performance of needle-shaped coke, combined with fiber and mosaic structure, the problems of needle-shaped coke have high resistivity, low charge and discharge efficiency and poor heat dissipation performance in high energy density lithium batteries are solved, and high Lithium-ion battery negative electrode material with fast charging performance and stable quality.

CN118978933APending Publication Date: 2024-11-19SHANDONG BINHE NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411188881.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The application of needle-shaped coke in high-energy and high-power density lithium batteries is limited by its high resistivity, low charging and discharging efficiency and poor heat dissipation performance, resulting in low battery charging efficiency and safety hazards, and the mixing of multiple raw materials is caused by Quality fluctuations affect product quality.

Method used

By selecting cycloalkyl reduced pressure heavy oil and catalytic oil slurry as the main raw materials, needle-shaped coke combining fiber and mosaic structure is prepared, its polarization structure and electrochemical performance are optimized, and the coking process is adopted to improve conductivity and heat dissipation performance and avoid raw materials The mass fluctuations caused by mixing and mixing.

Benefits of technology

Achieve high-capacity fast-charging lithium-ion battery negative electrode material, improves Li(+) diffusion rate and charging capacity retention rate, reduces heat accumulation, stabilizes product quality, and avoids mass fluctuations caused by mixing raw materials .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of high-performance materials, and particularly provides high-capacity fast-charging needle coke for a lithium ion battery negative electrode material, which is obtained by coking naphthenic base reduced pressure heavy oil and catalytic slurry oil as raw materials, the ratio of the naphthenic base reduced pressure heavy oil to the catalytic slurry oil is (1: 9)-(9: 1); the needle coke realizes the change of a polarization structure, is applied to the high-capacity fast-charging negative electrode material industry, not only keeps relatively high capacity, but also gives consideration to certain fast-charging performance, and can avoid the problem that the quality of a negative electrode material is fluctuated and the quality of a negative electrode material product is influenced due to the mixing of various raw materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of high-performance materials, and in particular relates to a high-capacity fast-charging needle coke used as a negative electrode material for lithium-ion batteries. Background Art

[0002] High-capacity fast-charging technology has developed rapidly in recent years, especially in the field of consumer electronics such as electric vehicles and smart phones. The widespread application of this technology has brought about a sharp increase in demand for battery materials, among which needle coke, as a key raw material for manufacturing high-performance lithium battery negative electrode materials, has become increasingly important.

[0003] Needle coke has high specific capacity performance characteristics and is an ideal material for manufacturing high energy density and high power density lithium batteries. With the popularization of high-capacity fast charging technology, the demand for needle coke is also increasing.

[0004] As an important battery material, needle coke has broad application prospects in the field of fast charging. However, in practical applications, needle coke still has some problems in fast charging, which limits its application in high energy density and high power density batteries. There are three major problems with needle coke in fast charging: 1. High resistivity and poor conductivity One of the main problems with needle coke is that it has a high resistivity and relatively poor conductivity, which results in a high internal resistance of the battery during fast charging, increased losses in converting electrical energy into heat, and reduced battery charging efficiency and energy density. Therefore, improving the conductivity of needle coke is one of the keys to solving the fast charging problem.

[0005] 2. Low charging and discharging efficiency The charge and discharge efficiency of needle coke is also an important factor that limits its fast charging performance. During fast charging, the battery needs to quickly charge and release a large amount of electrical energy, and the low charge and discharge efficiency of needle coke means that more electrical energy is wasted on resistance, resulting in a reduction in the actual available electrical energy. This not only affects the charging speed of the battery, but also reduces the overall performance of the battery.

[0006] 3. Severe fever and rapid temperature rise During fast charging, the battery will generate a certain amount of heat. However, the poor thermal conductivity of needle coke makes it impossible to dissipate the heat in time, causing the battery temperature to rise rapidly. High temperature not only affects the performance and life of the battery, but may also cause safety issues. Therefore, in fast charging applications, the heating problem of needle coke needs to be solved urgently.

[0007] Among negative electrode material customers, as the demands of end customers continue to increase, especially the requirements of new energy vehicles for long battery life and fast charging are clearly reflected, the long battery life brought by high capacity must also be compensated by fast charging performance in order to achieve better application of the product to customers. The solution of negative electrode material manufacturers to this kind of problem is to use high-capacity needle coke and other coke raw materials with certain fast charging performance for mixed use. It does have a certain effect during use, but there are also big problems: First, this kind of product is related to the volatility of two or more raw materials themselves, and there are fluctuations in product quality. Second, it is also related to the mixing technology used by different negative electrode customers, which leads to fluctuations in the quality of negative electrode materials, which ultimately affects the product quality of negative electrode materials and affects customer experience.

[0008] In summary, needle coke has problems in fast charging, such as high resistivity and poor conductivity, low charging and discharging efficiency, severe heat generation and rapid temperature rise. In order to give full play to the application potential of needle coke in the field of fast charging, it is necessary to further improve its conductivity, improve charging and discharging efficiency, and optimize heat dissipation performance. This will provide strong support for the development of needle coke in the field of fast charging. Summary of the invention

[0009] Needle coke is currently used in the lithium-ion battery negative electrode material industry. Due to the large number of needle coke fibers, the gram capacity is relatively high after application. The highest gram capacity of button cells produced can reach 362mAh / g. High capacity has become the greatest value of needle coke applications. However, the fiber structure accounts for a large proportion, the layered structure is relatively good, and the fast charging performance is affected.

[0010] The inventors further studied the polarized structure of needle coke, selected three different coke raw materials, and prepared them into artificial graphite negative electrode materials. The material structure and electrochemical properties were characterized and analyzed by polarizing microscope, X-ray diffraction analyzer, rate charging, electrochemical AC impedance spectroscopy and other methods. The research results show that the artificial graphite obtained from needle coke A composed of fiber and mosaic structure has good orientation, and the Li(+) diffusion in its pole piece is fast, and the capacity retention rate charged at 3 C is the highest, reaching 81.7%; the artificial graphite obtained from petroleum coke B composed of mosaic structure has good orientation, but the Li(+) diffusion in its pole piece is slow; and the artificial graphite obtained from needle coke C composed of fiber structure has the worst orientation, and the Li(+) diffusion in its pole piece is slow; the fast charging performance of artificial graphite materials obtained from B and C is poor. The inventors finally chose needle coke A composed of fiber and mosaic structure as the research direction.

[0011] Based on the above research, the inventors started from the direction in which raw materials affect the performance of coke, and finally chose cycloalkane vacuum heavy oil and catalytic oil slurry as the main raw materials, realizing the change of the polarization structure of needle-shaped coke, which is applied to the high-capacity fast-charging negative electrode material industry. It not only maintains a relatively high capacity, but also takes into account a certain fast-charging performance, and can avoid the quality fluctuations of negative electrode materials caused by the mixing of multiple raw materials, which affects the quality of negative electrode material products.

[0012] The high-capacity fast-charging needle coke for lithium-ion battery negative electrode materials provided in this scheme is mainly obtained after coking with cycloalkyl vacuum heavy oil and catalytic oil slurry as raw materials; the mass ratio of the cycloalkyl vacuum heavy oil and the catalytic oil slurry is 1:9-9:1.

[0013] Preferably, the mass ratio of the cycloalkane vacuum heavy oil to the catalytic oil slurry is 2:8 to 6:4.

[0014] Preferably, the ash content of the catalytic oil slurry is ≤0.05%, the total aromatics are 50-70%, and the sulfur content is 1.0-2.0%.

[0015] The naphthenic vacuum heavy oil contains 10-20% asphaltenes, 20-40% saturated hydrocarbons, 20-40% aromatic hydrocarbons, and the remainder is colloid.

[0016] Furthermore, the cycloalkane vacuum heavy oil has a sulfur content of ≤3.5%, an ash content of 0.05-0.2%, a carbon residue of ≤23%, and a density of ≤1.03 kg / m 3 .

[0017] In the selection process of cycloalkane vacuum heavy oil, it is necessary to analyze the characteristics of the four components of the raw materials and control the stable saturated hydrocarbons, aromatic hydrocarbons, asphaltenes and resins. From the component point of view, saturated hydrocarbons are relatively easy to react under thermal cracking conditions. When heated to high temperatures (such as above 450°C), saturated hydrocarbon molecules will crack and the large molecular chains will break into small molecular chains, mainly generating small molecular alkanes and olefins. This process is mainly carried out according to the free radical reaction mechanism. At high temperatures, the CC bonds in the hydrocarbon molecules break to form free radicals, which in turn trigger a series of chain reactions.

[0018] Aromatic hydrocarbons usually do not or rarely undergo ring-opening due to their good thermal stability. However, at high temperatures, aromatic hydrocarbons mainly undergo dealkylation and dehydrogenation condensation reactions. Dealkylation reactions shorten or even completely remove the alkyl side chain, while dehydrogenation condensation reactions may cause aromatic hydrocarbon molecules to connect to form larger molecules.

[0019] Asphaltene is the component with the largest molecular weight and the most complex structure in heavy oil. During the thermal cracking process, asphaltene molecules will undergo cracking reactions to generate small molecular hydrocarbons. At the same time, asphaltene may also undergo polymerization reactions, especially in the absence of water, high temperatures will promote its polymerization to form larger molecules.

[0020] Resin is a complex, highly polar component in heavy oil. During the thermal cracking process, resin will also undergo cracking reactions, mainly producing small molecular hydrocarbons. Similar to asphaltene, resin may also undergo polymerization reactions under anhydrous conditions.

[0021] Different microstructures have a significant impact on the electrochemical properties of coke. Aromatic hydrocarbons mainly provide layered fibrous structures for the structure of coke, while colloids and asphaltene mainly form coke quickly, and most of the structures formed are mosaic structures. During the reaction of saturated hydrocarbons, most of them are easy to break chains to produce small molecules, and a small amount of condensation is converted into large molecular weight components to generate fibrous and mosaic structure coke.

[0022] Catalytic oil slurry is a by-product produced by the catalytic device. The composition of the catalytic oil slurry also needs to be selected. Catalytic oil slurry is a high-aromatic substance, and the properties of the catalytic oil slurry produced by the refinery vary greatly. Generally, it contains a certain amount of ash. In the technical solution of this application, the catalyst powder is removed by pretreatment to control the product ash content to ≤0.05%; at the same time, the total aromatics are controlled at 50~70%, so as to better cooperate with cycloalkane vacuum heavy oil to form coke.

[0023] The preparation method of the needle coke comprises the following specific steps: After the cycloalkane vacuum heavy oil and catalytic oil slurry are fully mixed, they enter the heat exchange process and are heated by the coking furnace to a temperature of 480~515℃. After the coking conditions are met, they are sent to the coking tower. The coking pressure is controlled between 0.1~0.6Mpa, and the coking cycle is 36 or 48 hours to finally obtain the target needle coke.

[0024] The final needle coke has an ash content of ≤0.25wt%, sulfur ≤2.5wt%, and true density ≥1.36 g / cm 3 , the volatile matter is 5~12wt%, and the Harmo index is 60~100.

[0025] In the above preparation process, the coking tower (coking furnace) contains gaseous and liquid fraction products and circulating oil, among which the dry gas is used as fuel for the plant equipment, and the liquefied petroleum gas, light hydrocarbon by-products and heavy hydrocarbon by-products of coking can be supplied to the downstream for use.

[0026] The high-capacity fast-charging needle coke obtained by the above technical solution has the following technical effects: 1) In heavy oil, normal alkanes, cycloalkanes, and the side chains on cycloalkane rings and aromatic rings are all composed of four valence electron chain carbon atoms, and only aromatic rings are composed of aromatic carbon atoms with one π electron and three valence electrons. Aromatic ring radicals composed of aromatic carbon atoms will shrink into macromolecules and expand in the two-dimensional plane direction, while cycloalkane ring radicals composed of chain carbon atoms will expand in the three-dimensional direction when condensed into macromolecules. Chain carbon condensates have chemical chains combined horizontally and vertically. Therefore, coke synthesized by high condensation of condensed ring cycloalkanes is isotropic, and has different structures of spherical and needle-shaped. Therefore, the raw materials for high-quality coke need to be heavy oil with less chain carbon and cycloalkane carbon and more aromatic carbon.

[0027] In the coking reaction of aromatic-rich oil, as the degree of condensation deepens, the carbon content of the reactants continues to increase, the side chains gradually decrease, the aromatic ring surface continues to expand, the molecular weight becomes larger and larger, and the polycyclic compounds begin to condense together to form colloidal particles called micelles or molecular bundles. At the same time, there is a directional flattening or aligning effect between the aromatic rings of the planar structure. When the colloidal particles further condense to a certain extent, a crystal with a clear interface with the mother liquid will appear. It has both anisotropic solid properties and liquid properties that can flow and be spherical when suspended, so it is called the mesophase. The crystal separated from the mother liquid is called the mesophase sphere, and many polycyclic aromatic molecules are hierarchically gathered inside the sphere.

[0028] After adding cycloalkyl vacuum heavy oil, the polarized structure of coke changes significantly. The polarized structure of coke generated by thermal cracking of cycloalkyl vacuum heavy oil may show a more messy feature, which is mainly due to the complex chemical reactions and component changes in the thermal cracking process. The structure of this coke may not have obvious flow texture like needle coke, and may show a more complex texture and crystal structure, but its overall order may be lower. The polarized structure is coke with a mosaic structure, which mainly refers to isotropy. This optical structure is a state in which the mosaic structure and the small domain structure coexist. The production of vacuum heavy oil produced by adding cycloalkyl crude oil will add a part of the mosaic structure to the structure of the coke, and finally form a combination of fiber and mosaic structure. The fibrous structure of the catalytic oil slurry shows a flow texture. The combination of the two structures forms the advantages of high capacity and fast charging performance.

[0029] 2) Cycloalkane vacuum heavy oil is more reactive under thermal cracking conditions and more likely to form an isotropic structure. It is more likely to form an isotropic structure in needle coke, which increases the Li(+) diffusion channel.

[0030] 3) By preparing needle coke with fiber and inlaid structure, the problem of mixing different raw materials in the existing process to improve fast charging performance, which leads to fluctuations in the quality of negative electrode materials and affects product quality, is avoided. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further described below in conjunction with specific embodiments. These implementation cases are only used to illustrate the technical solution of the present invention in more detail and should not be understood as limiting the scope of protection of the present invention. Unless otherwise specified, the percentages in this application are all mass percentages; The catalytic oil slurry used in the following examples has an ash content of ≤0.05%, a total aromatic content of 50-70%, and a sulfur content of 1.0-2.0%; The naphthenic vacuum heavy oil contains 10-20% asphaltenes, 20-40% saturated hydrocarbons, 20-40% aromatic hydrocarbons, and the remainder is colloid; Furthermore, the cycloalkane vacuum heavy oil has a sulfur content of ≤3.5%, an ash content of 0.05-0.2%, a carbon residue of ≤23%, and a density of ≤1.03 kg / m 3 .

[0032] The above raw materials are all purchased directly from the market, and it is only necessary to control the purchased finished products to meet the above indicators.

[0033] Example 1 A high-capacity fast-charging needle coke for lithium-ion battery negative electrode material, the raw material composition of which is the above-mentioned catalytic oil slurry and cycloalkane vacuum heavy oil, and the mass ratio of the two is 1:9.

[0034] The preparation method of the needle coke comprises the following specific steps: After the cycloalkane vacuum heavy oil and catalytic oil slurry are fully mixed, they enter the heat exchange process and are heated by the coking furnace to a temperature of 480~505℃. After the coking conditions are met, they are sent to the coking tower. The coking pressure is controlled between 0.1~0.4Mpa, and the coking cycle is 48 hours, and the target needle coke is finally obtained.

[0035] The final needle coke has an ash content of ≤0.25wt%, sulfur ≤2.5wt%, and a true density of 1.36~1.38g / cm 3 The volatile matter is 7.5~8.5wt% and the Harmo index is 65~95.

[0036] Example 2

[0037] A high-capacity fast-charging needle coke for lithium-ion battery negative electrode material, the raw material composition of which is the above-mentioned catalytic oil slurry and cycloalkane vacuum heavy oil, and the mass ratio of the two is 9:1.

[0038] The preparation method of the needle coke comprises the following specific steps: After the cycloalkane vacuum heavy oil and catalytic oil slurry are fully mixed, they enter the heat exchange process and are heated by the coking furnace to a temperature of 485~515℃. After the coking conditions are met, they are sent to the coking tower. The coking pressure is controlled between 0.2~0.6Mpa, and the coking cycle is 48 hours, and the target needle coke is finally obtained.

[0039] The final needle coke has an ash content of ≤0.15wt%, sulfur ≤2.5wt%, and a true density of 1.4~1.41g / cm 3 , the volatile matter is 5~7wt%, and the Harmo index is 65~85.

[0040] Example 3

[0041] A high-capacity fast-charging needle coke for lithium-ion battery negative electrode material, the raw material composition of which is the above-mentioned catalytic oil slurry and cycloalkane vacuum heavy oil, and the mass ratio of the two is 3:7.

[0042] The preparation method of the needle coke comprises the following specific steps: After the cycloalkane vacuum heavy oil and catalytic oil slurry are fully mixed, they enter the heat exchange process and are heated by the coking furnace to a temperature of 480~505℃. After the coking conditions are met, they are sent to the coking tower. The coking pressure is controlled between 0.1~0.4Mpa, and the coking cycle is 48 hours, and the target needle coke is finally obtained.

[0043] The final needle coke has an ash content of ≤0.25wt%, sulfur ≤2.5wt%, and a true density of 1.38~1.39g / cm 3 , the volatile matter is 7~8wt%, and the Harmo index is 75~95.

[0044] Example 4

[0045] A high-capacity fast-charging needle coke for lithium-ion battery negative electrode material, the raw material composition of which is the above-mentioned catalytic oil slurry and cycloalkane vacuum heavy oil, and the mass ratio of the two is 7:3.

[0046] The preparation method of the needle coke comprises the following specific steps: After the cycloalkane vacuum heavy oil and catalytic oil slurry are fully mixed, they enter the heat exchange process and are heated by the coking furnace to a temperature of 485~510℃. After the coking conditions are met, they are sent to the coking tower. The coking pressure is controlled between 0.2~0.5Mpa, and the coking cycle is 48 hours, and the target needle coke is finally obtained.

[0047] The final needle coke has an ash content of ≤0.15wt%, sulfur ≤2.5wt%, and a true density of 1.39~1.40g / cm 3 , the volatile matter is 6~7.5wt%, and the Harmo index is 70~85.

[0048] Comparative Example 1 The technical solution of Example 2 is adopted, except that only catalytic oil slurry is used as raw material.

[0049] The final needle coke has an ash content of ≤0.1wt%, sulfur ≤1.0wt%, and a true density of 1.38~1.41g / cm 3 , the volatile matter is 5.5~7wt%, and the Harmo index is 75~85.

[0050] The needle coke obtained in Example 2 and Comparative Example 1 was made into a lithium-ion battery graphite negative electrode material that complies with GB / T 24533-2009 according to the existing conventional process, and finally made into a button cell and then subjected to relevant performance testing. The results are shown in Table 1 below: Table 1 .

[0051] According to the above table, the negative electrode material prepared from needle coke prepared in Example 2 has basically no decrease in true density, compaction, capacity and first efficiency, but has a significant improvement in charge rate, which fully demonstrates that Example 2 not only maintains a relatively high capacity compared with Comparative Example 1 in terms of performance, but also takes into account a certain fast charging performance, and avoids the problem of negative electrode material quality fluctuations caused by the mixing of multiple raw materials adopted by current negative electrode material manufacturers, which affects the quality of negative electrode material products, and the effect is significant.

[0052] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any equivalent substitutions, modifications, etc. made by technicians in this field without any creative work within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-capacity fast-charging needle coke for lithium-ion battery negative electrode material, characterized in that: The invention is obtained by coking cycloalkyl vacuum heavy oil and catalytic oil slurry as raw materials; the ratio of the cycloalkyl vacuum heavy oil and the catalytic oil slurry is 1:9-9:1; the needle coke has an ash content of ≤0.25wt%, a sulfur content of ≤2.5wt%, and a true density of ≥1.36 g / cm 3 , the volatile matter is 5~12wt%, and the Harmo index is 60~100.

2. The high-capacity fast-charging needle coke for lithium-ion battery negative electrode material according to claim 1, characterized in that: The mass ratio of the cycloalkane vacuum heavy oil to the catalytic oil slurry is 2:8 to 6:

4.

3. The high-capacity fast-charging needle coke for lithium-ion battery negative electrode material according to claim 1 or 2, characterized in that: The ash content of the catalytic oil slurry is ≤0.05%, the total aromatics content is 50-70%, and the sulfur content is 1.0-2.0%.

4. The high-capacity fast-charging needle coke for lithium-ion battery negative electrode material according to claim 1 or 2, characterized in that: The naphthenic vacuum heavy oil contains 10-20% asphaltenes, 20-40% saturated hydrocarbons, 20-40% aromatic hydrocarbons, and the remainder is colloid.

5. The high-capacity fast-charging needle coke for lithium-ion battery negative electrode material according to claim 1 or 2, characterized in that: The cycloalkane vacuum heavy oil has a sulfur content of ≤3.5%, an ash content of 0.05-0.2%, a carbon residue of ≤23%, and a density of ≤1.03 kg / m 3 .

6. The method for preparing high-capacity fast-charging needle coke for lithium-ion battery negative electrode material according to claim 1, characterized in that: The specific steps are as follows: After the cycloalkane vacuum heavy oil and catalytic oil slurry are fully mixed, they enter the heat exchange process and are heated by the coking furnace to a temperature of 480~515℃. After the coking conditions are met, they are sent to the coking tower. The coking pressure is controlled at 0.1~0.6Mpa and the coking time is 36~48 hours to finally obtain the target needle coke.