Desulfurization protective agent as well as preparation method and application thereof
Through the preparation method of desulfurization protection agent with red mud as raw material, the problems of low utilization rate of red mud and high cost of blast furnace gas desulfurization protection agent in alumina production are solved, and the resource utilization of red mud and efficient removal of acidic substances are achieved.
Patent Information
- Application Number
- CN202411410379.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-19
AI Technical Summary
The utilization rate of large amounts of red mud produced in alumina production is low, resulting in environmental pollution, and the protective agent used in the deacidification process in blast furnace gas essence desulfurization technology is high.
Using a desulfurization protective agent with red mud as the main raw material, it is prepared by combining dry-mixed materials, binder and water through steps such as drying, grinding, mixing, extrusion molding and roasting to form an efficient acid removal substance. desulfurization protector.
Effectively absorbing red mud produced in alumina production, reducing environmental pollution, and cost lower than traditional protective agents, achieving effective removal of acidic substances in blast furnace gas, and realizing the resource utilization of red mud.
Smart Images

Figure CN118978940A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource recycling, and in particular to a desulfurization protective agent and a preparation method thereof. Background Art
[0002] Red mud is the solid waste discharged from the production of alumina. It is highly alkaline and radioactive and is a polluting waste. About 1.0-2.5 tons of red mud are discharged for every ton of alumina produced. According to the calculation that 1.5 tons of red mud are discharged for every ton of alumina produced, the annual red mud discharge is as high as hundreds of millions of tons. At present, the utilization rate of red mud in my country is only about 6%. Most alumina plants use open-air dams to store red mud. This method not only occupies a large amount of land and wastes resources, but the alkali in it will also penetrate into the ground, causing groundwater and soil pollution; the dust formed by the exposed red mud will pollute the atmosphere, have adverse effects on the survival of humans, animals and plants, and deteriorate the ecological environment. Therefore, it is a difficult problem that the aluminum industry needs to solve urgently to reasonably absorb the large amount of red mud generated in the process of alumina production and alleviate environmental pollution.
[0003] At the same time, the process flow dominated by the desulfurization technology of the steel industry is a three-stage treatment system of deacidification-hydrolysis-desulfurization, in which the deacidification process uses alkaline porous materials to remove acidic substances in blast furnace gas, the hydrolysis process converts carbonyl sulfide (COS) in blast furnace gas into H2S, and the desulfurization process removes H2S in the gas. The deacidification process plays a vital role in the entire stage. To ensure that the subsequent catalyst is not poisoned by acidic substances, a protective agent is required. At present, the protective agent is prepared by porous materials loaded with alkaline substances, which is relatively expensive and sold for more than 10,000 yuan, resulting in high operating costs for blast furnace gas.
[0004] Therefore, how to use red mud to provide a desulfurization protective agent to reduce the cost of blast furnace gas desulfurization is a problem that technicians in this field urgently need to solve. Summary of the invention
[0005] In view of this, the present invention provides a protective agent to solve the problems of large amount of red mud produced and low utilization rate in the existing aluminum industry, and high cost of the protective agent used in the deacidification process in the blast furnace gas fine desulfurization technology.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] On the one hand, the present invention provides a desulfurization protective agent, including a dry mixed material, a binder and water; in terms of mass percentage, the dry mixed material includes 90-95% red mud, 5-10% pore-forming agent and 0-5% structural additive; the amount of the binder added is 2-10% of the mass of the dry mixed material, and the amount of water added is 15-35% of the mass of the dry mixed material.
[0008] Preferably, the dry mixed material further comprises a structural additive, and the added amount of the structural additive is 0-5% of the mass of the dry mixed material.
[0009] Preferably, the structural additive includes at least one of cement and fly ash.
[0010] Preferably, the pore-forming agent includes at least one of ammonium bicarbonate and starch.
[0011] Preferably, the binder includes at least one of polyvinyl alcohol, sodium silicate, sodium carboxymethyl cellulose, carboxymethyl cellulose, guar gum and bentonite.
[0012] Preferably, the mass content of calcium oxide in the red mud is ≥20%.
[0013] On the other hand, the present invention also provides a method for preparing the desulfurization protective agent described in any one of the above, comprising the following steps:
[0014] (1) drying, grinding and then sieving the red mud to obtain red mud powder;
[0015] (2) mixing the red mud powder, pore former and structure additive to obtain a dry mixed material;
[0016] (3) mixing the dry mixed material, the binder and water and extruding the mixture to obtain a precursor;
[0017] (4) Post-treating the precursor to obtain a desulfurization protective agent.
[0018] Preferably, the drying temperature in step (1) is 110-200° C., and the drying time is 2-24 h.
[0019] Preferably, the particle size of the red mud powder in step (1) is 0.074-0.15 mm.
[0020] Preferably, the post-treatment in step (4) is calcination at ≤ 900° C. for 5-10 h.
[0021] Preferably, the precursor is spherical or strip-shaped, and the diameter of the precursor is 1-6 mm.
[0022] Furthermore, the present invention also provides a use of the desulfurization protective agent described in any one of the above items or the desulfurization protective agent prepared by any one of the above preparation methods in the fine desulfurization of blast furnace gas.
[0023] The present invention provides a desulfurization protective agent, which has the following beneficial effects compared with the prior art:
[0024] The desulfurization protective agent of the present invention uses red mud as the main raw material, can absorb a large amount of red mud generated in the alumina production process, and effectively alleviates environmental pollution; the preparation method of the desulfurization protective agent of the present invention is simple, no waste is generated in the whole process and the cost is low. Using it in the blast furnace gas fine desulfurization process can effectively remove acidic substances in the blast furnace gas, and realize the resource utilization of red mud in the aluminum industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0026] Figure 1 This is a physical picture of the desulfurization protective agent of the present invention;
[0027] Figure 2 It is a comparison chart of COS conversion rate under the action of the desulfurization protective agent of the present invention and the traditional desulfurization protective agent;
[0028] Figure 3 It is the XRD diagram before and after the industrial side line reaction of the desulfurization protective agent of the present invention. DETAILED DESCRIPTION
[0029] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the reagents and equipment used are all commercially available. If in the following examples, specific treatment conditions and treatment methods are not clearly described, then conditions and methods known in the art can be used to process.
[0030] In one aspect of the present invention, the present invention proposes a desulfurization protective agent, comprising a dry mixed material, a binder and water; wherein, in terms of mass percentage, the dry mixed material comprises 90-95% of red mud, 5-10% of a pore former and 0-5% of a structural additive; the amount of the binder added is 2-10% of the mass of the dry mixed material, and the amount of water added is 15-35% of the mass of the dry mixed material.
[0031] In the present invention, the dry mixed material comprises 90-95% red mud, specifically 90%, 91%, 92%, 93%, 94% and 95% red mud, in terms of mass percentage. Preferably, the mass content of calcium oxide in the red mud is ≥ 20%. Calcium oxide is the active ingredient of the deacidifier in the blast furnace gas fine desulfurization technology. If the content is too low, the removal rate of acidic substances in the blast furnace gas is unqualified.
[0032] In the present invention, the dry mixed material includes 5-10% of the pore former in terms of mass percentage, specifically 5%, 6%, 7%, 8%, 9% and 10% of the pore former. Preferably, the pore former includes at least one of ammonium bicarbonate and starch. The main function of the pore former is to produce a pore structure in the material. In the subsequent heat treatment process, the pore former is easily decomposed under heating conditions, releasing gas and overflowing from the protective agent, thereby leaving a pore structure inside the desulfurization protective agent and increasing the specific surface area of the desulfurization protective agent.
[0033] In the present invention, the dry mixed material includes 0-5% of structural additives in terms of mass percentage, and specifically can be 1%, 2%, 3%, 4%, 5%, etc. of structural additives. Preferably, the structural additive includes at least one of cement and fly ash. In the present invention, the structural additive is an optional component to be added, and its main function is to enhance the strength of the desulfurization protective agent. Specifically, the alkali in the red mud acts as an alkali activator, reacts with the Si-containing substance in the structural additive, and forms a geopolymer, thereby achieving the purpose of enhancing the strength of the desulfurization protective agent.
[0034] In the present invention, the amount of the binder added is 2-10% of the mass of the dry mixed material, specifically 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% and 10% of the binder. Preferably, the binder includes at least one of polyvinyl alcohol, sodium silicate, sodium carboxymethyl cellulose, carboxymethyl cellulose, guar gum and bentonite, wherein if the amount of the binder added is too low, the strength of the prepared desulfurization protective agent is too low, and if the amount of the binder added is too large, the humidity is too high and it is difficult to form.
[0035] In the present invention, the amount of water added is 15-35% of the mass of the dry mixed material, specifically 15%, 20%, 25%, 30%, 35% of water, so as to dissolve the binder.
[0036] On the other hand, the present invention also provides a method for preparing the protective agent described in any one of the above, comprising the following steps:
[0037] Step S100: drying, grinding and sieving the red mud to obtain red mud powder.
[0038] The present invention has no particular limitation on the drying method, as long as the red mud can be dried.
[0039] In the present invention, it is preferred to dry the red mud to a water content of ≤20%, for example, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, etc. The original water content of the red mud has little effect on the effect of the final protective agent, but if the original water content of the red mud is too high (greater than 20%), "hanging material phenomenon" will occur during the red mud breakage and grinding process. In the actual production process, it is necessary to pay attention to the original red mud water content at all times, and adjust the amount of water added during kneading according to the red mud water content at all times to ensure that the water content during kneading is 30-35%. At this time, the product strength obtained is better.
[0040] In some embodiments of the present invention, the drying temperature in step (1) is 110-200°C, and the drying time is 2-24h. For example, it can be dried at 110°C for 24h, dried at 150°C for 10h, dried at 200°C for 2h, etc.
[0041] The present invention does not specifically limit the specific method of grinding, as long as the red mud powder of the particle size required for subsequent grinding can be obtained. In an embodiment of the present invention, it is preferred to grind the dried red mud and sieve it to a particle size of 0.074-0.15 mm. Among them, the red mud powder ground to 0.074-0.15 mm accounts for 60-70% of the total powder ratio and can be sieved. The red mud powder is sieved to a particle size of 0.074-0.15 mm, for example, 0.074 mm, 0.080 mm, 0.090 mm, 0.10 mm, 0.12 mm, 0.13 mm, 0.15 mm, etc. If the particle size of the red mud powder is too large, it is easy to block the holes in the extrusion process and it is not easy to extrude.
[0042] Step S200: Mix the red mud powder, pore former and structural additive to obtain a dry mixed material.
[0043] The present invention has no particular limitation on the mixing method, as long as the red mud powder and the pore-forming agent can be mixed evenly.
[0044] Step S300: Mix the dry mixed material, binder and water and extrude them to obtain a precursor.
[0045] The precursor obtained in the present invention is spherical or strip-shaped, and the diameter of the precursor is 1-6 mm, for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, etc. If the precursor is strip-shaped, the length is generally controlled to be 2-3 cm, for example, 2 cm, 2.5 cm, 3 cm, etc.
[0046] In the present invention, the dry mixed material, the binder and the water are mixed and kneaded, and the precursor is obtained after the mud kneading and extrusion process. The water content during kneading is controlled to be 30-35%, for example, it can be 30%, 31%, 32%, 33%, 34%, 35%, etc. At this time, the extrusion strength is high. If the water content is too low, the extruded protective agent is hard and obviously pulverized. If it is too high, the extruded protective agent is too soft and sticks to each other. Extrusion can be a strip extrusion or granulation operation to obtain a strip or spherical precursor. The present invention does not specifically limit the specific processes of kneading, mud kneading and extrusion.
[0047] (4) Post-treating the precursor to obtain a desulfurization protective agent.
[0048] The heat treatment of the present invention is calcining for 5-10 hours at ≤900°C in an air atmosphere, for example, calcining at 300°C for 10 hours, 500°C for 7 hours, 800°C for 5 hours, etc. The post-treatment process can remove the water contained in the protective agent to leave the surface of the protective agent, thereby enhancing the strength of the protective agent. On the other hand, the pore-forming agent can be volatilized in the post-treatment process, leaving the pore structure to increase the specific surface area of the protective agent. If the calcination temperature is too low, the pore-forming agent cannot be effectively volatilized, and if the calcination temperature is too high, the active components in the red mud will volatilize, affecting the use effect of the protective agent.
[0049] The process of preparing the desulfurization protective agent by using red mud as raw material is simple, does not require a large amount of equipment investment, and the production cost of each ton of desulfurization protective agent can be controlled within 3,000 yuan, which is much lower than 10,000 yuan of traditional commercially available protective agents. The cost is low and industrial mass production can be realized.
[0050] The present invention also provides a use of any of the above-mentioned desulfurization protective agents or the desulfurization protective agent prepared by any of the above-mentioned preparation methods in the fine desulfurization of blast furnace gas.
[0051] The technical solution of the present invention is described in detail below through specific embodiments.
[0052] It should be noted that the conventional desulfurization protective agent involved below is a potassium carbonate product supported on an alumina carrier, and the strength of the conventional desulfurization protective agent is 80-100 N / cm.
[0053] Example 1
[0054] (1) drying aluminum industrial red mud with a calcium oxide content of 26% at 110° C. for 24 hours, wherein the water content of the dried red mud is 3%, grinding and sieving the dried red mud to obtain red mud powder with a particle size of 0.075-0.15 mm;
[0055] (2) dry-mixing red mud powder, cement and ammonium bicarbonate in a mass ratio of 90:5:5 to obtain a dry mixed material;
[0056] (3) After mixing polyvinyl alcohol and dry mixed materials, distilled water is added to the mixture until the water content is 32%, and the mixture is kneaded, kneaded, and extruded to obtain a precursor; wherein the amount of polyvinyl alcohol added is 5% of the mass of the dry mixed materials, and the amount of distilled water added is 15% of the mass of the dry mixed materials;
[0057] (4) In an air atmosphere, the precursor obtained in step (3) is calcined at 300° C. for 5 h to obtain a blast furnace gas fine desulfurization protective agent.
[0058] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in Example 1 could reach 96% of the protective effect of the traditional desulfurization protective agent, and the strength was 62 N / cm.
[0059] Example 2
[0060] (1) drying aluminum industrial red mud with a calcium oxide content of 26% at 200° C. for 2 h, wherein the water content of the dried red mud is 2.4%, grinding and sieving the dried red mud to obtain red mud powder with a particle size of 0.075-0.15 mm;
[0061] (2) dry-mixing red mud powder and ammonium bicarbonate in a mass ratio of 95:5 to obtain a dry mixed material;
[0062] (3) After mixing polyvinyl alcohol and dry mixed materials, distilled water is added to the mixture until the water content is 31%, and the mixture is kneaded, kneaded, and extruded to obtain a precursor; wherein the amount of polyvinyl alcohol added is 5% of the mass of the dry mixed materials, and the amount of distilled water added is 35% of the mass of the dry mixed materials;
[0063] (4) In an air atmosphere, the precursor obtained in step (3) is calcined at 300° C. for 5 h to obtain a blast furnace gas fine desulfurization protective agent.
[0064] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in Example 2 could reach 72.3% of the protective effect of the traditional desulfurization protective agent, and the strength was 42.19 N / cm.
[0065] Example 3
[0066] (1) drying aluminum industrial red mud with a calcium oxide content of 26% at 110° C. for 10 h, wherein the water content of the dried red mud is 3%, grinding and sieving the dried red mud to obtain red mud powder with a particle size of 0.075-0.15 mm;
[0067] (2) dry-mixing red mud powder, cement and ammonium bicarbonate in a mass ratio of 90:4:6 to obtain a dry mixed material;
[0068] (3) After mixing polyvinyl alcohol and dry mixed materials, distilled water is added to the mixture until the water content is 30%, and the mixture is kneaded, kneaded, and extruded to obtain a precursor; wherein the amount of polyvinyl alcohol added is 5% of the mass of the dry mixed materials, and the amount of distilled water added is 20% of the mass of the dry mixed materials;
[0069] (4) In an air atmosphere, the precursor obtained in step (3) is calcined at 300° C. for 5 h to obtain a blast furnace gas fine desulfurization protective agent.
[0070] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in Example 3 could reach 87.5% of the protective effect of the traditional desulfurization protective agent, and the strength was 77.90 N / cm.
[0071] Example 4
[0072] (1) drying aluminum industry red mud with a calcium oxide content of 26% at 150° C. for 15 h, wherein the water content of the dried red mud is 3%, grinding and sieving the dried red mud to obtain red mud powder with a particle size of 0.075-0.15 mm;
[0073] (2) dry-mixing red mud powder, fly ash and starch in a mass ratio of 90:2:8 to obtain a dry-mixed material;
[0074] (3) After mixing sodium silicate and dry mixed materials, distilled water is added to the mixture until the water content is 35%, and the mixture is kneaded, slurried, and extruded to obtain a precursor; wherein the amount of sodium silicate added is 5% of the mass of the dry mixed materials, and the amount of distilled water added is 15% of the mass of the dry mixed materials;
[0075] (4) In an air atmosphere, the precursor obtained in step (3) is calcined at 400° C. for 5 h to obtain a blast furnace gas fine desulfurization protective agent.
[0076] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in Example 4 could reach 91.4% of the protective effect of the traditional desulfurization protective agent, and the strength was 75.86 N / cm.
[0077] Example 5
[0078] (1) drying aluminum industrial red mud having a calcium oxide content of 30% at 110° C. for 15 h, wherein the water content of the dried red mud is 5%, grinding and sieving the dried red mud to obtain red mud powder of 0.075-0.15 mm;
[0079] (2) dry-mixing red mud powder, cement and starch in a mass ratio of 92:3:5 to obtain a dry-mixed material;
[0080] (3) After mixing polyvinyl alcohol and dry mixed materials, distilled water is added to the mixture until the water content is 34%, and the mixture is kneaded, kneaded, and extruded to obtain a precursor; wherein the amount of polyvinyl alcohol added is 5% of the mass of the dry mixed materials, and the amount of distilled water added is 20% of the mass of the dry mixed materials;
[0081] (4) In an air atmosphere, the precursor obtained in step (3) is calcined at 800° C. for 10 h to obtain a blast furnace gas fine desulfurization protective agent.
[0082] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in Example 5 can reach 96% of the protective effect of the traditional desulfurization protective agent, and the strength is 68.00 N / cm.
[0083] like Figure 1 , 2 , 3 are related diagrams of the desulfurization protective agent prepared in Example 5 of the present invention. Figure 1 This is a physical picture of the desulfurization protective agent of the present invention. It can be seen from the figure that the desulfurization protective agent prepared by using red mud in the present invention has no powder falling phenomenon and has high strength; Figure 2 The figure is a comparison chart of the COS conversion rate of the desulfurization protective agent of the present invention and the traditional desulfurization protective agent. It can be seen from the figure that the COS conversion rate of the protective agent of the present invention is equivalent to the COS conversion rate of the traditional protective agent; Figure 3 The figures are the XRD diagrams before and after the industrial side-line reaction of the protective agent of the present invention, wherein a and c are the X-ray diffraction diagrams before the reaction of the red mud-based protective agent, and b and d are the X-ray diffraction diagrams after the reaction of the protective agent. It can be seen from the figures that the Ca element in the red mud exists as alkaline substances such as Ca(OH)2 and CaCO3, and is the main active substance for removing HCl from blast furnace gas. Comparing the figures a and c, the Ca(OH)2 diffraction peaks in b and d are significantly reduced, indicating that it participates in the reaction during the process.
[0084] The test method of COS conversion rate is as follows: adopt industrial side-line test, introduce industrial gas into two parallel reaction tubes, and -1 Under the conditions of temperature of 110°C and carbonyl sulfide hydrolysis catalyst, one reaction tube was filled with a traditional protective agent and the other reaction tube was filled with a desulfurization protective agent. The COS conversion rate was evaluated at regular intervals, and the evaluation cycle was 50 hours.
[0085] Example 6
[0086] (1) drying aluminum industrial red mud having a calcium oxide content of 26% at 110° C. for 10 h, wherein the water content of the dried red mud is 4%, grinding and sieving the dried red mud to obtain red mud powder of 0.075-0.15 mm;
[0087] (2) dry-mixing red mud powder, fly ash and starch in a mass ratio of 90:5:5 to obtain a dry mixed material;
[0088] (3) After mixing sodium silicate and dry mixed materials, distilled water is added to the mixture until the water content is 35%, and the mixture is kneaded, kneaded, and extruded to obtain a precursor; wherein the amount of sodium silicate added is 5% of the mass of the dry mixed materials, and the amount of distilled water added is 20% of the mass of the dry mixed materials;
[0089] (4) In an air atmosphere, the precursor obtained in step (3) is calcined at 500° C. for 6 h to obtain a blast furnace gas fine desulfurization protective agent.
[0090] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in Example 6 could reach 81.5% of the protective effect of the traditional desulfurization protective agent, and the strength was 77.90 N / cm.
[0091] Example 7
[0092] This embodiment is basically the same as Embodiment 1, the only difference being that the red mud from the aluminum industry is not dried before grinding and has a water content of 15%.
[0093] The industrial side-line test was used for evaluation. Within a test evaluation period of 50 hours, the protective effect of the protective agent prepared in this embodiment can reach 95% of the protective effect of the traditional desulfurization protective agent, and the strength is 60N / cm.
[0094] Example 8
[0095] This embodiment is substantially the same as embodiment 1, the only difference being that the protective agent precursor is heat treated at 150° C. for 5 h.
[0096] The industrial side-line test was used for evaluation. Within a test evaluation period of 50 hours, the protective effect of the protective agent prepared in this embodiment can reach 92.6% of the protective effect of the traditional desulfurization protective agent, and the strength is 70.84 N / cm.
[0097] Example 9
[0098] This embodiment is substantially the same as embodiment 1, the only difference being that the protective agent precursor is heat treated at 900° C. for 5 h.
[0099] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in this embodiment can reach 95% of the protective effect of the traditional desulfurization protective agent, and the strength is 70.63N / cm.
[0100] Example 9
[0101] This embodiment is basically the same as Embodiment 1, the only difference being that the protective agent precursor is dried in sunlight for 10 hours.
[0102] The industrial side-line test was used for evaluation. Within a test evaluation period of 50 hours, the protective effect of the protective agent prepared in this embodiment can reach 90.6% of the protective effect of the traditional desulfurization protective agent, and the strength is 73N / cm.
[0103] Comparative Example 1
[0104] This comparative example is substantially the same as Example 1, except that the red mud powder, cement and ammonium bicarbonate are dry-mixed in a mass ratio of 90:7:3.
[0105] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in Example 2 can reach 68.24% of the protective effect of the traditional desulfurization protective agent, and the strength is 102N / cm.
[0106] Comparative Example 2
[0107] This comparative example is substantially the same as Example 1, except that the amount of polyvinyl alcohol added is 1% of the mass of the dry mixed material.
[0108] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in Example 3 can reach 90.24% of the protective effect of the traditional desulfurization protective agent, and the strength is 36.32 N / cm.
[0109] Comparative Example 3
[0110] This embodiment is substantially the same as embodiment 1, the only difference being that the protective agent precursor is heat treated at 1000° C. for 5 h.
[0111] The industrial side-line test was used for evaluation. Within the test evaluation period of 50 hours, the protective effect of the protective agent prepared in Example 5 can reach 82% of the protective effect of the traditional desulfurization protective agent, and the strength is 42N / cm.
[0112] From Comparative Examples 1 to 3, it can be seen that
[0113] (1) Adding structural additives during the preparation of the protective agent can improve its strength, but it will also reduce the content of active components in the protective agent. Therefore, during the preparation of the protective agent, attention should be paid to the balance between strength and adsorption performance of the protective agent.
[0114] (2) In the process of preparing the protective agent, the amount of binder added is related to the strength of the protective agent. In the actual production process, if the amount of binder added is too small, the protective agent cannot be formed into a certain shape. If the amount of binder added is too large, the mixed material will stick to the surface of the machine and cannot be formed.
[0115] (3) In the process of preparing the desulfurization protective agent, if the heat treatment temperature is too high, the active components in the red mud will evaporate, and the protective effect and strength of the desulfurization protective agent finally prepared will be reduced.
[0116] In summary, the present invention uses red mud from the aluminum industry to prepare a blast furnace gas fine desulfurization protective agent, and uses the alkali in the red mud to remove the acidic substances in the blast furnace gas, providing a high-value utilization route for large-scale stockpiled red mud solid waste, and no waste water and other wastes are generated during the entire production process. The alkalinity of the red mud protective agent after use is greatly reduced, and it can be used as a common building material for resource utilization.
[0117] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A desulfurization protective agent, It is characterized in that Includes dry mix, binder and water; Calculated by mass percentage, the dry mixed material includes 90-95% of red mud, 5-10% of pore former and 0-5% of structural additive; The amount of the binder added is 2-10% of the mass of the dry mixed material, and the amount of water added is 15-35% of the mass of the dry mixed material.
2. The desulfurization protective agent according to claim 1, It is characterized in that The structural additive includes at least one of cement and fly ash.
3. The desulfurization protective agent according to claim 1, It is characterized in that The pore-forming agent includes at least one of ammonium bicarbonate and starch.
4. The desulfurization protective agent according to claim 1, It is characterized in that The binder includes at least one of polyvinyl alcohol, sodium silicate, sodium carboxymethyl cellulose, carboxymethyl cellulose, guar gum and bentonite.
5. The desulfurization protective agent according to any one of claims 1 to 4, It is characterized in that The mass content of calcium oxide in the red mud is ≥20%.
6. A method for preparing the desulfurization protective agent according to any one of claims 1 to 5, It is characterized in that The following steps are involved: (1) drying, grinding and then sieving the red mud to obtain red mud powder; (2) mixing the red mud powder, pore former and structure additive to obtain a dry mixed material; (3) mixing the dry mixed material, the binder and water and extruding the mixture to obtain a precursor; (4) Post-treating the precursor to obtain a desulfurization protective agent.
7. The method for preparing the desulfurization protective agent according to claim 6, It is characterized in that The drying temperature in step (1) is 110-200° C. and the drying time is 2-24 h; The particle size of the red mud powder is 0.074-0.15 mm.
8. The method for preparing the desulfurization protective agent according to claim 6, It is characterized in that The post-treatment in step (4) is calcination at ≤900°C for 5-10h.
9. A method for preparing a desulfurization protective agent according to any one of claims 6 to 8, It is characterized in that The precursor is in a spherical or strip shape, and the diameter of the precursor is 1-6 mm.
10. Use of the desulfurization protective agent according to any one of claims 1 to 5 or the desulfurization protective agent prepared by the preparation method according to any one of claims 6 to 9 in the fine desulfurization of blast furnace gas.